Technical Details of Sealing and Solder Glass Frits

SCHOTT offers more than 100 SCHOTT standard glass types, different wet/dry grinding methods, and patented technologies that come together to form a wide range of exceptionally durable glass powder products. SCHOTT translates specific physical and chemical requirements into tailor-made solutions for a variety of challenging applications.

Superior sealants from a world leader in specialty glass

Superior resistance to harsh elements

Sealing and solder glasses produced by SCHOTT offer a variety of beneficial properties, including chemical resistance in highly corrosive conditions and outstanding stability in extreme operating temperatures of up to 1,040°C.

Reproducible high purity

To achieve the stable high quality our customers expect, our sealing and solder glasses are produced in dedicated melting and grinding facilities. We can provide all levels of output, from sample quantities to mass production.

Sub-micron particle size

SCHOTT glass frits are available in a wide range of particle size distributions, from an average particle size of 2,000 µm down to special submicron grinds.

R&D and production partnership

By working with SCHOTT, you benefit from close technical support and long-term supply security from a trusted and established supplier. We also provide active local support through our international presence.

Specifications

Please refer to the tables below to choose the right sealing glass for your desired combination of materials. SCHOTT has a wide range of sealing glasses available in a number of different grain sizes.

 

Sealing Glasses for High Temperature Applications

Sealing Partner SCHOTT Glass Number  CTE* (10-6/K for 20-300 °C) Tg ( °C )  Sealing temperature( °C )  Maximum operating temperature ( °C ) 
 SiC 8253  4.6  785 1320  735 
AIN G018-200 4.6 557 665  550
 AI2O3 G018-266 6.9 585  770 530
G018-346  7.3  720  1270  670 
G018-358

8.5

8.8**

685 940 

600

1040**

G018-385
8.4** 992**  950  950 °C ( 1000)
 ZrO2 G018-339  9.2**  627 990 760** 
G018-311

9.1

9.9**

622 850

560

880**

 

*CTE = coefficient of thermal expansion    **p.c. = partially crystalline

 

SOFC and SOEC Sealing Glasses 

Glass No.  α20/300)[ppm/K]*
Tg [°C] Dil. Ew [°C] p [g/cm3] Sealing temperature [ °C] Sealing partners
GM31107 9.8 543  592 3.70 700 Crofer, ITM, StS
G018-281 12.1 639 > 850 2.70  1000 CFY
G018-311
9.9 612 686 3.80 850  Crofer, ITM, StS
G018-354
9.2 637  711 3.90 850 Crofer, ITM, StS
G018-381
12.1 652  > 850 2.30 950 CFY 
G018-385
8.4 992 >1000 3.14 1000 CFY
 

*p.c. = partially crystalline

SCHOTT Solder Glasses

The choice of solder glass for joining different materials is dependent on four major aspects:

  • Desired soldering temperature
  • Thermal expansion of the materials to be joined
  • Operation temperature of the final application
  • Chemical behavior

Please refer to the table below for details on standard SCHOTT solder glass types. We have a wide range of solder glasses available in a number of different grain sizes.

Glass No. α(20/300) (10-6 x K-1)
Tg [ °C ]* Sealing temperature [ °C ] Sealing temperature tholding [min] Density [g/cm3] tk100[ °C ] tanδ [ 10-4 ]
Lead-containing
 G017-002 3.7 545 700  15  3.6  - 37
G017-339
4.7 325 510 15 4.3 11.5 19
G017-712
5.3  375 510 10 -  -  -
G017-393
6.5 320 425 15 4.8 11.6  15
G017-340
7.0 315 420 15 4.8 13.4 14
G018-228
7.6 311 400  15 5.0 - -
8465 8.2 385 520 60 5.4 14.9 27
G018-229  8.7 310 410 15 5.4 - -
G018-256
9.6 316 420 15 5.8 - -
G017-052
11.7 308 410 15  6.7 - -
Lead-free
G018-250
7.0 380 540 15 5.7 - -
G018-255
9.4 396 520 15  6.7 - -
8470 10.0 440 680 60 2.8 - -
G018-249
10.1 365 500 15 7.1 - -
 
Other matched CTE available upon customer request. 

All glass frits are available as K3 powder. Grain size: d50 = 10 +- αµm, d99 ≤ 63µm

Other grain sizes available upon request.

Want to know more? Let's talk

Whether you need more information, samples, a quote, or advice for a project, I would be delighted to talk to you.

Contact us
Weston Wright.jpg

Weston Wright

Product Sales Manager