Technical Details of B 270®
Market-leading transmittance and thickness range
Material properties of B 270®
1. Optical properties
Optical Properties | Value |
---|---|
Refractive index* ng | 1.5341 |
Refractive index* nF' | 1.5297 |
Refractive index* nF | 1.5292 |
Refractive index* ne | 1.5251 ± 0.001 |
Refractive index* nd | 1.5230 |
Refractive index* nD | 1.5229 |
Refractive index* nC' | 1.5207 |
Refractive index* nC | 1.5203 |
Abbe value νe | 58.3 ± 0.6 |
Photoelastic constant in (nm/cm)/Mpa | 27.5 |
2. Thermal properties
General thermal properties | Unit | Value |
---|---|---|
Mean specific heat capacity cp | in J/(g·K) (20 °C ; 100 °C) | 0.8 |
Transformation temperature Tg | in °C | 542 |
"Coefficient of thermal Expansion (CTE) α in 10-6·K-1 (static measurement)"
Degree | Value |
---|---|
(20 °C; 300 °C) | 9.4 |
(20 °C; 200 °C) | 9.0 |
(20 °C; 100 °C) | 8.6 |
"Coefficient of thermal Expansion (CTE) α in 10-6·K-1 (dynamic measurement)"
Degree | Value |
---|---|
(20 °C; 100 °C) | 8.6 |
(20 °C; 150 °C) | 8.8 |
(20 °C; 200 °C) | 9.0 |
(20 °C; 250 °C) | 9.2 |
(20 °C; 300 °C) | 9.4 |
(20 °C; 350 °C) | 9.6 |
(20 °C; 400 °C) | 9.7 |
(20 °C; 450 °C) | 9.9 |
Viscosities | Viscosity lg ŋ in dPas | Temperature in °C |
---|---|---|
Strain point | 14.5 | 507 |
Annealing point | 13.0 | 535 |
Softening point | 7.6 | 711 |
Fuseability:
Fusing with SCHOTT ARTISTA® glasstypes using an adapted temperature / time programme results in a technically stressfree compound with a maximum stress birefringence of 70 nm/cm.
3. Mechanical properties
Mechanical Properties |
Unit | Value |
---|---|---|
Density ρ | in g/cm³ | 2.56 |
Young's modulus E | in kN/mm² | 71.1 |
Poisson's ratio µ | 0.22 | |
Torsion modulus G | in kN/mm² | 29 |
Knoop hardness | HK 0.1/20 | 500 |
Vickers hardness | HV 0.2/25 | 510 |
Chemical toughening (for thickness = 2.0 mm)
Unit |
Value |
---|---|
Temperature ϑ in °C | 410 |
Time t in h | 4 |
Compressive stress (CS) in MPa | 441 |
Depth of layer (DoL) in µm | 11 |
Thermal Toughening
Thermal toughening of B 270® is possible
4. Chemical properties
Hydrolytic resistance (acc. to DIN ISO 719) | Value |
---|---|
Class | HGB 3 |
Equivalent of alkali per gram glass grains in µg/g | 136 |
Acid resistance (acc. to DIN 12116) | Value |
---|---|
Class | S 2 |
Half surface weight loss after 6 hours in mg/dm² | 0.7 |
Alkali resistance (acc. to DIN ISO 695) | Value |
---|---|
Class | A 1 |
Surface weight loss after 3 hours in mg/dm² | 71 |
5. Electrical properties
Dielectric constant εr (at ϑ = 25 °C) | Value |
---|---|
at 1 MHz | 7.5 |
at 1 GHz | 6.7 |
at 2 GHz | 6.8 |
at 5 GHz | 6.7 |
at 24 GHz | 6.6 |
Dissipation factor tan δ (at ϑ = 25 °C) |
Value |
---|---|
at 1 MHz | 32 · 10-4 |
at 1 GHz | 59 · 10-4 |
at 2 GHz | 66 · 10-4 |
at 5 GHz | 84 · 10-4 |
at 24 GHz | 150 · 10-4 |
Electric volume resistivity ρD in Ω·cm (at 50 Hz) |
---|
6.1 · 107 ( ϑ = 250 °C) |
1.6 · 106 (ϑ = 350 °C) |
6. Transmittance values
Spectral transmittance 250 - 3200 nm
Spectral transmittance 250 - 450 nm
Wavelength in nm at thickness 2.0 mm: | τ (λ) in % |
---|---|
254 | < 0.1 |
380 | 90.8 |
632.8 | 91.9 |
1064 | 91.8 |
Edge wavelength at 2 mm thickness | Wavelength in nm |
---|---|
λc (τ = 0.46) | 310 |
λS ( τ = 0.05) | 293 |
λP ( τ = 0.85) | 338 |
Solarization* after UV-radiation at 2 mm thickness | Δ λc in nm |
---|---|
Shifting of the UV edge wavelength λc (τ = 0.46) in the direction of longer wavelength | < 2 |
*Measuring and Test Procedures
The sample will be irradiated with a UV - F 400 flood lamp.
The irradiation time amounts to 7h; the distance between flood lamp and sample fastening is 14 cm.
Luminous transmittance at thickness in mm | τvD65 in % | τvA in % |
---|---|---|
2.0 | 91.7 | 91.7 |
UV - transmittance at thickness in mm | τUVA in % | τUVB in % |
---|---|---|
2.0 | 84 | 19 |
IR – transmittance at thickness in mm | τA in % |
---|---|
2.0 | 91.9 |
Solar direct transmittance at thickness | τe in % |
---|---|
2.0 | 91.6 |
7. Colorimetry
Chromaticity coordinates* at thickness 2.0 mm | Value |
---|---|
D65 | x = 0.313 |
D65 | y = 0.329 |
A | x = 0.448 |
A | y = 0.408 |
General color rendering index Ra at thickness in mm | Value |
---|---|
2.0 | 100 |
* Chromaticity coordinates (color locus) are referred to the named Standard Illuminant according to CIE (2°-Observer)
Material properties of B 270® Thin
1. Optical
Optical properties | Value |
---|---|
Refractive index* ng | 1.5341 |
Refractive index* nF' | 1.5297 |
Refractive index* nF | 1.5292 |
Refractive index* ne | 1.5251 ± 0.001 |
Refractive index* nd | 1.5230 |
Refractive index* nD | 1.5229 |
Refractive index* nC' | 1.5207 |
Refractive index* nC | 1.5203 |
Abbe valueνe | 58.3 ± 0.6 |
Photoelastic constant in (nm/cm)/Mpa | 28.6 |
* Refractive indices:
Pretreatment of samples. Condition as supplied ["as drawn"]
2. Thermal
General thermal properties | Unit | Value |
---|---|---|
CTE (Coefficient of thermal expansion) α | 10-6·K-1 (20 °C; 300 °C) | 9.4 |
Mean specific heat capacity cp | in J/(g·K) (20 °C ; 100 °C) | 0.8 |
Transformation temperature Tg | in °C | 536 |
Viscosities | Viscosity lg ŋ in dPas | Temperature in °C |
---|---|---|
Strain point | 14.5 | 505 |
Annealing point | 13.0 | 535 |
Softening point | 7.6 | 723 |
3. Mechanical
Mechanical properties |
Unit | Value |
---|---|---|
Densityρ | in g/cm³ | 2.56 |
Young's modulus E | in kN/mm² | 69.8 |
Poisson's ratio µ | 0.25 | |
Torsion modulus G | in kN/mm² | 28 |
Knoop hardness | HK 0.1/20 | 480 |
Vickers hardness | HV 0.2/25 | 520 |
Chemical toughening (for thickness = 0.3 mm)
Unit | Value |
---|---|
Temperatureϑin °C | 410 |
Time t in h | 4 |
Compressive stress (CS) in MPa | 331 |
Depth of layer (DoL) in µm | 16 |
4. Chemical
Hydrolytic resistance (acc. to DIN ISO 719) | Value |
---|---|
Class | HGB 3 |
Equivalent of alkali per gram glass grains in µg/g | 170 |
Acid resistance (acc. to DIN 12116) | Value |
---|---|
Class | S 2 |
Half surface weight loss after 6 hours in mg/dm² | 1.0 |
Alkali resistance (acc. to DIN ISO 695) | Value |
---|---|
Class | A 2 |
Surface weight loss after 3 hours in mg/dm² | 80 |
5. Electrical
Dielectric constant εr (at ϑ= 25 °C) | Value |
---|---|
at 1 MHz | 7.2 |
at 1 GHz | 6.8 |
at 2 GHz |
6.8 |
at 5 GHz | 6.7 |
at 24 GHz |
6.8 |
at 77 GHz | 6.5 |
Dissipation factor tanδ (atϑ= 25 °C) |
Value |
---|---|
at 1 MHz | 32 · 10-4 |
at 1 GHz | 59 · 10-4 |
at 2 GHz |
66 · 10-4 |
at 5 GHz | 84 · 10-4 |
at 24 GHz | 150 · 10-4 |
at 77 GHz | 230 · 10-4 |
Conductivity σ in S/cm for direct current | Value |
---|---|
at 25 °C | 5 · 10-16 |
at 250 °C | 4 · 10-9 |
at 350 °C | 2 · 10-7 |
Electric volume resistivity ρD in Ω·cm for alternating current 50 Hz | Value |
---|---|
at 25 °C | 8.6 · 1011 |
at 250 °C | 2.4 · 108 |
at 350 °C | 5.8 · 106 |
Temperature tk 100 in °C | Value |
---|---|
at 108 Ω · cm | 272 |
6. Transmittance values
Spectral transmittance 250 - 3050 nm
Spectral Transmittance: 250 - 450 nm
Wavelength in nm at thickness 0.3 mm: | τ(λ) in % |
---|---|
254 | < 0.1 |
380 | 91.3 |
632.8 | 92.0 |
1064 | 92.2 |
Edge wavelength λc (τ = 0.46) at thickness in mm | Wavelength in nm |
---|---|
0.3 | 287 |
0.9 | 299 |
Luminous transmittance at thickness in mm | τvD65 in % | τvA in % |
---|---|---|
0.3 | 91.9 | 91.9 |
0.9 | 91.6 | 91.7 |
B 270® products
SCHOTT B 270® is available as:
- Sheets
- Cut-to-size substrates
- Polished substrates and wafers
SCHOTT B 270® Thin is available as:
- Cut-to-size substrates
- Unpolished substrates and wafers
To find out more, please see the related products on the overview page.