Does this match your preferences? Make a selection.

ZERODUR® Low thermal expansion glass-ceramic

ZERODUR® glass-ceramic has been one of SCHOTT's most unique and extraordinary products for over 50 years. With an extremely low thermal expansion, it's essential for a large number of demanding high-tech applications requiring exceptional precision.

Download technical specs
a piece of ZERODUR® low thermal expansion glass-ceramic
Overview

    Blue magnifying glass icon, symbolizing search or zoom functionality. A window into distant galaxies

    SCHOTT ZERODUR® glass-ceramic ensures that crisp images are available to unlock mysteries of the cosmos with the world's largest telescope.

    Info.svg Enabling the future of gravitational-wave astronomy

    With the LISA Pathfinder mission, the European Space Agency (ESA) paved the way for the first space-based observatory of gravitational waves. At its core: ZERODUR® glass-ceramic.

    Award & innovation Expert insights on ZERODUR®

    Explore dedicated ZERODUR® training content covering ultra-low expansion glass-ceramics, optical system design, astronomy applications and precision engineering.

    *Required field

    SCHOTT will only use your data to respond to your inquiry. For more information, please click here.

    Hexagon-shaped ZERODUR® glass-ceramic by SCHOTT

    Highly accurate under extreme conditions

    The extremely low thermal expansion of ZERODUR® glass-ceramic is homogenous throughout the entire bulk volume, which makes it ideal for a large range of applications involving precise positioning or imaging under changing temperature conditions.
    Disc of ZERODUR® glass-ceramic for telescope mirror

    Impressive machinability from small to large

    Thanks to its extraordinary machining properties, ZERODUR® can be manufactured in a variety of sizes and shapes, from tiny prisms to meter-sized mirror blanks. High degree light-weighting and surfaces optimized for bending strength are key areas of SCHOTT's expertise, which makes ZERODUR® ideal for space applications.
    Dr. Florian Kanal, Business Development and Strategic Marketing
    For over 50 years, ZERODUR® has helped engineers push the limits of precision. If your application demands stability, reliability, and performance, we're ready to face your challenge.
    Technical details

    Technical details of ZERODUR®

    For several decades, the unique technical properties of ZERODUR® glass-ceramic have made it ideal for a vast range of applications that rely on exceptionally low thermal expansion materials. It's also now the industry standard for ultra-precise mirror substrates in astronomy.

    CTE tolerances of ZERODUR®

    By default, the mean coefficient of thermal expansion (CTE) of ZERODUR® is measured within the temperature range of 0°C to 50°C. Five expansion classes are differentiated as follows:

    CTE Grades

    CTE (0°C; 50°C)*

    ZERODUR® Expansion Class 2

    0 ± 0.100 ・ 10-6/K

    ZERODUR® Expansion Class 1

    0 ± 0.050 ・ 10-6/K

    ZERODUR® Expansion Class 0

    0 ± 0.020 ・ 10-6/K

    ZERODUR® Expansion Class 0 SPECIAL

    0 ± 0.010 ・ 10-6/K

    ZERODUR® Expansion Class 0 EXTREME

    0 ± 0.007 ・ 10-6/K

    ZERODUR® TAILORED

    TAILORED ± 0.020・10-6/K 
    (± 0.010・10-6/K upon request) 
    Optimized for application temperature

    *CTE (0°C; 50°C) describes the linear mean coefficient of thermal expansion in the temperature 0°C to 50°C.

     

    Maximum application temperature 600°C.

    Upon request, ZERODUR® is available for customized temperature ranges.

    We offer expansion class 0 or better optimized for your individual application.

     

    CTE homogeneity

    Homogeneity is evaluated by measuring CTE samples homogeneously distributed throughout the blank and calculating the difference in CTE between the highest and the lowest value measured.

    The homogeneity of linear expansion can be guaranteed in the following weight classes:

    CTE (0°C; 50°C) Homogeneity Tolerances

    • up to 18 tons: < 0.03 ・ 10-6/K

    • up to 6 tons: < 0.02 ・ 10-6/K

    • up to 0.3 tons: < 0.01 ・ 10-6/K

     

    CTE distribution within a 1.5 m diameter blank with a measured CTE homogeneity of 0.004 · 10-6/K

    CTE distribution map within a 1.5 m diameter ZERODUR® blank

     

    CTE tolerances of ZERODUR® K20

    ZERODUR® K20, a high-temperature version of ZERODUR®, has been optimized to withstand higher application temperatures.

    Mean coefficient of linear thermal expansion of ZERODUR® K20

    • CTE (20°C; 700°C): 2.4・10-6/K

    • CTE (20°C; 300°C): 2.2・10-6/K

    • CTE (0°C; 50°C): 1.6 ・ 10-6/K

    Maximum application temperature 850°C.

    If no quality is specified upon receipt of an order, then ZERODUR® will be supplied in standard quality. Individual specifications for internal quality can be fulfilled upon request.

    Inclusions

    Although the defect level is low, the main inclusions found in ZERODUR® are bubbles. During inspection of ZERODUR® parts, all inclusions with a diameter > 0.3 mm are taken into consideration. If an inclusion has a shape other than spherical, the average diameter is reported as the mean of the length and width. ZERODUR® is available in six different inclusion quality levels, which are defined according to the dimension of your part.

    Quality levels for inclusions in ZERODUR®

    Average number of inclusions per 100 cm3:

    Standard

    5.0

    Class 4

    5.0 

    Class 3

    4.0

    Class 2

    3.0

    Class 1

    2.0

    Class 0

    1.0

     

    Maximum diameter of individual inclusions in mm for different diameters or diagonals of the ZERODUR® part:

    In the critical volume

    < 500 mm 

    < 2000 mm

    < 4000 mm 

    Standard

    1.4

    2.0 

    3.0 

    Class 4

    1.2 

    1.8 

    2.5 

    Class 3

    1.0

    1.6 

    2.0 

    Class 2

    0.8

    1.5 

    1.8 

    Class 1

    0.6

    1.2 

    1.6 

    Class 0

    0.4

    1.0 

    1.5 

     

    In the uncritical volume

    < 500 mm

    < 2000 mm

    < 4000 mm

    Standard

    3.0

     6.0

    10.0

    Class 4

    2.0

    5.0 

    8.0 

    Class 3

    1.5

    4.0 

    6.0 

    Class 2

    1.0

    3.0 

    6.0 

    Class 1

    0.8

    3.0 

    6.0 

    Class 0

    0.6

    3.0 

    6.0 

    Individual specifications upon request.

     

    Bulk stress

    The bulk stress birefringence of ZERODUR® is recorded in path difference per thickness in inspection direction. For discs it is measured in axial direction at 5 % of the diameter from the edge. For rectangular plates, the measurement is performed in the middle of the longer side perpendicular to the plate‘s surface.

    Quality levels for bulk stress in ZERODUR®

    Bulk stress birefringence [nm/cm] for parts with diameters or diagonals:

     

    < 500 mm

    < 2000 mm 

    < 4000 mm

    Standard

    6        

    12       

    15       

    Class 4

    4

    10

    12

    Individual specifications upon request

     

    Striae

    Additionally to the bulk stress birefringence, the stress birefringence induced by local striae is classified as a function of part diameter.

    Stress birefringence caused by striae [nm/striae] for parts with diameters or diagonals:

     

    < 500 mm

    < 2000 mm 

    < 4000 mm

    Standard

    60 

    60 

    60 

    Class 4 

    45

    45 

    45 

    Class 3

    30 

    30 

    30 

    Class 2 

    5 

    30 

    30 

    Class 1 

    - 

    5 

    30 

    ZERODUR® is processed into complex geometries based on technical drawings and specifications from our customers. Our application and process engineers support you during the design phase of your product to get the most out of the ZERODUR® properties for your individual application. We also provide finite-element modelling and special quality requirements upon request.

    5-axis CNC grinding machines allow for precise fabrication of ZERODUR® parts up to 4.25 m in diameter. The highlight of ZERODUR® processing is its light-weighting by grinding challenging aspect ratios of pocket heights to rib thickness used for parts with strict weight requirements.

    By single-side and double-side polishing, we offer different surface-quality grades for dimensions up to 500 mm. Depending on the size of your part, a roughness down to the sub-nanometer range can be achieved.

    As ZERODUR® acts as a very good substrate for coating, several coatings from standard aluminum to complex customized coatings are available for parts smaller than 300 mm. Our coating experts are ready to support you in choosing the coating that matches your specifications best.

     

    Proposed CNC grinding tolerances for dimensions and shapes

    Dimension < 2000 mm 

    Tolerances [mm]

    Thighter tolerances [mm]*

    Length, width, height

    ± 0.3

    ± 0.1

    Diameter

    ± 0.3

    ± 0.1

    Angle

    ± 5’

    ± 1’

    Flatness **

    0.1 - 0.2

    0.1

    Cylindricity **

    0.1

    0.1

    Profile **

    0.2

    0.1

    Parallelism **

    0.1 - 0.2

     0.1 

    Position **

    0.1

    0.1

    Concentricity **

    0.1

    0.1

    Run-out **

    0.1

    0.1

    * tighter tolerances depend on the size and geometry. They cannot be combined freely.

    ** according ISO 1101

     

    Dimension ≤ 4000 mm

    Tolerances [mm]

    Thighter tolerances [mm]*

    Length, width, height

    ± 0.4

    ± 0.2

    Diameter

    ± 0.4

    ± 0.2 

    Angle

    ± 5’

    ± 1’

    Flatness **

    0.2

    0.1 

    Cylindricity **

    0.2

    0.1

    Profile **

    0.4

    0.2

    Parallelism **

    0.2

    0.1

    Position **

    0.2

    0.1

    Concentricity **

    0.2

    0.1

    Run-out **

    0.2

    0.1

    * tighter tolerances depend on the size and geometry. They cannot be combined freely.

    ** according ISO 1101

    Bending stress and lifetime calculation

    ZERODUR® is the material of choice when it comes to excellent thermal properties and precision in high-tech applications. Often these applications also require to withstand certain mechanical loads, such as continuously as in telescope mirror holders or short-term during rocket launch.

    The key factor to be evaluated to quantify the breakage stress of ZERODUR® is the surface quality, especially the occurrence of microcracks. In general, applying loads below 10 MPa tensile stress does not demand any special breakage analysis of ZERODUR®.

    SCHOTT’s exhaustive data on the breakage events of ground ZERODUR® samples has shown that it can withstand long-term (tens of years) mechanical loads of 30 to 100 MPa. This is much higher than previously predicted. Using a three-parameter Weibull distribution, we are happy to discuss the ZERODUR® lifetime under your individual long-term mechanical loads.

     

    Typical mechanical and optical properties

    ZERODUR®

    ZERODUR® K20

    Thermal conductivity λ at 20°C [W/(m・K)]

    1.46

    1.63

    Thermal diffusivity index a at 20°C [10-6m2/s]

    0.72

    -

    Heat capacity cp at 20°C [J/(g · K)]

    0.80

    0.90

    Young's modulus E at 20°C [GPa]-mean value

    90.3

    84.7

    Poisson‘s ratio

    0.24

    0.25

    Density ρ [g/cm3]

    2.53

    2.53

    Knoop Hardness HK 0.1/20 (ISO9385)

    620

    620

    Refractive index nd

    1.5424

    -

    Abbe number νd

    56.1

    -

    Internal transmittance Ti at 580 nm / 5 mm thickness

    0.95

    -

    Internal transmittance Ti at 580 nm / 10 mm thickness

    0.9

    -

    Stress optical coefficient K at λ = 589.3 nm [10-6MPa-1]

    3

    -

    Electrical resistivity ρ at 20°C [Ω · cm]

    2.6 · 1013

    -

    Tk100 [°C], Temperature for ρ = 108 [Ω · cm]

    178

    -

    At room temperature, most acids, alkalis, salts and dye solutions leave no residual traces on ZERODUR® surfaces. It can be etched by hydrofluoric acid as well as concentrated sulfuric acid at elevated temperatures. Furthermore, construction materials such as mica, chamotte, MgO and SiO2 do not react noticeably with ZERODUR® (up to 600°C for 5 h). By contrast, enamel reacts above 560°C by having its surface destroyed. 

    Based on the good chemical resistance of the material, coatings such as mirrors are removable in a reproducible manner. The polished surface is simply cleaned and recoated by an optimized protocol.

     

    Typical chemical properties

     

    ZERODUR®

    ZERODUR® K20

    Hydrolytic resistance class (ISO 719)

    HGB 1

     -

    Acid resistance class (ISO 8424)

    1.0

     -

    Alkali resistance class (ISO 10629)

    1.0

     -

    Climate resistance

    Class 1

     -

    Stain resistance

    Class 0

     -

    Helium permeability [Atoms/(cm · s · bar)] at 20°C

    1.6 · 106

     -

    Helium permeability [Atoms/(cm · s · bar)] at 100°C

    5.0 · 107

     -

    Helium permeability [Atoms/(cm · s · bar)] at 200°C

    7.2 · 108

     -

    FAQs

    ZERODUR® combines near-zero thermal expansion and exceptional homogeneity, making it ideal for applications where precision must remain unchanged over time and temperature.

    Even small temperature changes can cause materials to expand or contract. ZERODUR® minimizes these effects, helping optical and measurement systems maintain accuracy under changing environmental conditions.

    ZERODUR® is used in space optics, astronomical telescopes, semiconductor lithography, metrology systems, ring laser gyroscopes, and other high-precision applications.

    Yes. Different expansion classes and tailored material variants allow ZERODUR® to be optimized for specific temperature ranges and performance requirements.

    Yes. Advanced CNC machining enables complex 3D geometries, lightweighted mirror structures, drilled features, and application-specific designs while maintaining exceptional precision.

    Depending on the design, ZERODUR® mirror substrates can be lightweighted by up to 90% while maintaining excellent stiffness and dimensional stability.

    Download
    Downloads

    Downloads for ZERODUR®

    Want to know more? Let’s talk.

    Applications

    Applications of ZERODUR®

    When it comes to precision and homogeneity, ZERODUR® low thermal expansion glass-ceramic is the material of choice for a wide variety of high-tech applications. From performing vital roles in navigation systems to improving the performance of microchips, ZERODUR® continually evolves with each challenge.
    The ESO’s ELT (Extremely Large Telescope) observatory on the Cerro Armazones mountain in Chile

    Taking astronomy to the next level

    ZERODUR® is used for telescope mirror substrates in monolithic and segmented telescopes. As well as low thermal expansion (any fluctuation in temperature due to environmental changes would obfuscate telescope images), the easy machinability and polishing properties of ZERODUR® make it ideal for adaptive optics. This is why it was used to produce the 40 m segmented primary mirror in the Extremely Large Telescope (ELT) in Chile.

    Satellite orbiting a red planet

    Out of this world

    Space applications such as astronomy and earth observation require light and strong materials. ZERODUR® light-weighted mirror substrates withstand strong forces during satellite launch and already orbit our home planet as part of satellites such as Hubble and Chandra. Furthermore, its radiation-resistance and SCHOTT's ability to predict its breakage make ZERODUR® perfect for longtime space missions.

    Precision probe sensor on industrial metalworking equipment

    Supporting engineering masterpieces

    Extremely precise measurement and analysis of distances and geometrical shapes is an application for which the resistance to temperature fluctuations of ZERODUR®  is optimally suited in different industrial manufacturing processes. Scales and gauges manufactured from ZERODUR enable precise measurements of smallest distances in encoders for linear length measurements up to several meters, e.g. for correctly positioning axes within CNC milling machines and coordinate-measurement equipment. Robots for automation and manufacturing can reliably be positioned with the help of rotary encoders allowing precise measurement of the angle within the robot joint.

    Interior of an aircraft cabin with illuminated controls and displays

    Better navigation in the air

    Special laser cavities, mirror blanks and tiny prisms made from ZERODUR® are part of ring laser gyroscope (RLG), which are at the heart of the inertial navigation systems used in aircraft. These customized components enable a highly precise reference system thanks to their robustness, long lifetime and low gas permeability.

    M-101316

    Precision on the nano scale

    Miniaturization in integrated circuit (IC) systems requires very precise lithography and wafer positioning, which ZERODUR®‘s very low thermal expansion is ideally suited for. Additionally, the lithographical optics to create high resolution pixel patterns for OLED and LCD displays make use of this attribute.

    Markus Kissler-Patig, Senior Astronomer at the European Southern Observatory
    A project like the ELT would not be possible if a material such as ZERODUR® glass-ceramic did not exist.
    Product variants

    Product variants of ZERODUR®

    SCHOTT ZERODUR® can be optimized for specialist applications depending on customer requirements. We also manufacture several variants of the product, including ZERODUR® K20 and ZERODUR® TAILORED.

    Contact

    Want to know more? Let's talk!

    Whether you need more information, samples, a quote, or advice for a project, I would be delighted to talk to you.

    Man in glasses in business office on phone while working on laptop_330x190.jpg

    1 Step 1
    2
    3

    *Required field

    SCHOTT will only use your data to respond to your inquiry. For more information, please click here.

    Want to know more? Let's talk!

    Please send any questions or requests by using the contact form.