SCHOTT Advanced Optics offers a variety of radiation resistant glass types with different dispersion properties. These glass types are well-suited to use in surroundings with high radioactivity.
Technical Details
Refractive Indices
| Characteristics | λ [nm] | |
|---|---|---|
| n2,325.4 | 2,325.4 | 1.56416 |
| n1,970.1 | 1,970.1 | 1.56890 |
| n1,529.6 | 1,529.6 | 1.57419 |
| n1,060.0 | 1,060.0 | 1.58045 |
| nt | 1,014.0 | 1.58125 |
| ns | 852.1 | 1.58477 |
| nr | 706.5 | 1.58970 |
| nC | 656.3 | 1.59214 |
| nC' | 643.8 | 1.59284 |
| Characteristics | λ [nm] | |
|---|---|---|
| n632.8 | 632.8 | 1.59349 |
| nD | 589.3 | 1.59642 |
| nd | 587.6 | 1.59655 |
| ne | 546.1 | 1.60010 |
| nF | 486.1 | 1.60710 |
| nF' | 480.0 | 1.60799 |
| ng | 435.8 | 1.61578 |
| nh | 404.7 | 1.62330 |
| ni | 365.0 | |
| Characteristics | λ [nm] | |
|---|---|---|
| n334.1 | 334.1 | |
| n312.6 | 312.6 | |
| n296.7 | 296.7 | |
| n280.4 | 280.4 | |
| n248.3 | 248.3 | |
Internal Transmittance
| Characteristics | λ [nm] | |
|---|---|---|
| τ25/2500 | 2,500 | 0.200 |
| τ25/2325 | 2,325 | 0.316 |
| τ25/1970 | 1,970 | 0.707 |
| τ25/1530 | 1,530 | 0.979 |
| τ25/1060 | 1,060 | 0.998 |
| τ25/700 | 700 | 0.993 |
| τ25/660 | 660 | 0.987 |
| τ25/620 | 620 | 0.983 |
| τ25/580 | 580 | 0.977 |
| τ25/546 | 546 | 0.966 |
| τ25/500 | 500 | 0.934 |
| τ25/460 | 460 | 0.832 |
| τ25/436 | 436 | 0.612 |
| τ25/420 | 420 | 0.350 |
| τ25/405 | 405 | 0.090 |
| τ25/400 | 400 | 0.040 |
| τ25/390 | 390 | |
| τ25/380 | 380 | |
| τ25/370 | 370 | |
| τ25/365 | 365 | |
| τ25/350 | 350 | |
| τ25/334 | 334 | |
| τ25/320 | 320 | |
| τ25/310 | 310 | |
| τ25/300 | 300 | |
| τ25/290 | 290 | |
| τ25/280 | 280 | |
| τ25/270 | 270 | |
| τ25/260 | 260 | |
| τ25/250 | 250 | |
| Characteristics | λ [nm] | |
|---|---|---|
| τ10/2500 | 2,500 | 0.525 |
| τ10/2325 | 2,325 | 0.631 |
| τ10/1970 | 1,970 | 0.870 |
| τ10/1530 | 1,530 | 0.992 |
| τ10/1060 | 1,060 | 0.999 |
| τ10/700 | 700 | 0.997 |
| τ10/660 | 660 | 0.995 |
| τ10/620 | 620 | 0.993 |
| τ10/580 | 580 | 0.991 |
| τ10/546 | 546 | 0.986 |
| τ10/500 | 500 | 0.973 |
| τ10/460 | 460 | 0.929 |
| τ10/436 | 436 | 0.822 |
| τ10/420 | 420 | 0.657 |
| τ10/405 | 405 | 0.382 |
| τ10/400 | 400 | 0.276 |
| τ10/390 | 390 | 0.090 |
| τ10/380 | 380 | |
| τ10/370 | 370 | |
| τ10/365 | 365 | |
| τ10/350 | 350 | |
| τ10/334 | 334 | |
| τ10/320 | 320 | |
| τ10/310 | 310 | |
| τ10/300 | 300 | |
| τ10/290 | 290 | |
| τ10/280 | 280 | |
| τ10/270 | 270 | |
| τ10/260 | 260 | |
| τ10/250 | 250 | |
Partial Dispersion
| Characteristics | |
|---|---|
| Ps,t | 0.2355 |
| PC,s | 0.4930 |
| Pd,C | 0.2946 |
| Pe,d | 0.2370 |
| Pg,F | 0.5803 |
| Pi,h | |
| P's,t | 0.2324 |
| P'C',s | 0.5322 |
| P'd,C' | 0.2451 |
| P'e,d | 0.2339 |
| P'g,F' | 0.5139 |
| P'i,h | |
| Characteristics | |
|---|---|
| ΔPC,t | -0.0056 |
| ΔPC,s | -0.0028 |
| ΔPF,e | 0.0009 |
| ΔPg,F | 0.0036 |
| ΔPi,g | |
Downloads
Collection Datasheets
Catalog
TIE‘s - Technical Information
TIE-04: Test Report for Delivery Lots of Optical Glass-May 2016
PDF
200 kB
TIE-19: Temperature coefficient of Refractive Index-July 2016
PDF
414 kB
TIE-25: Striae in Optical Glass-June 2006
PDF
1.84 MB
TIE-26: Homogeneity of Optical Glass-February 2016
PDF
1.44 MB
TIE-27: Stress in Optical Glass-July 2004
PDF
694 kB
TIE-28: Bubbles and Inclusions in Optical Glass-May 2016
PDF
205 kB
TIE-29: Refractive Index and Dispersion-February 2016
PDF
1.89 MB
TIE-30: Chemical properties of Optical Glass-February 2016
PDF
128 kB
TIE-31: Mechanical and Thermal Properties of Optical Glass-July 2004
PDF
222 kB
TIE-32: Thermal Loads on Optical Glass-August 2004
PDF
252 kB
TIE-33: Bending Strength of Optical Glass and ZERODUR®-December 2015
PDF
2.71 MB
TIE-35: Transmittance of Optical Glass-October 2005
PDF
762 kB
TIE-36: Fluorescence of Optical Glass (EN)
PDF
710 kB
TIE-40: Optical Glass for Precision Molding-September 2011
PDF
526 kB
TIE-41: Large Optical Glass Blanks-September 2006
PDF
498 kB
TIE-42: Radiation Resistant Optical Glasses-April 2018
PDF
365 kB