SF57

Glass Code:  847238.551

A classic glass type with lead oxide as an essential component for outstanding optical properties.

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.84666 νd 23.83
ne 1.85504 νe 23.64
nF-nC 0.035536 nF'-nC' 0.036166
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.79026
n1,970.1 1,970.1 1.79539
n1,529.6 1,529.6 1.80187
n1,060.0 1,060.0 1.81185
nt 1,014.0 1.81335
ns 852.1 1.82038
nr 706.5 1.83102
nC 656.3 1.83650
nC' 643.8 1.83808
Characteristics λ [nm]
n632.8 632.8 1.83957
nD 589.3 1.84636
nd 587.6 1.84666
ne 546.1 1.85504
nF 486.1 1.87204
nF' 480.0 1.87425
ng 435.8 1.89393
nh 404.7 1.91366
ni 365.0
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.750
τ25/2325 2,325 0.790
τ25/1970 1,970 0.930
τ25/1530 1,530 0.991
τ25/1060 1,060 0.997
τ25/700 700 0.996
τ25/660 660 0.994
τ25/620 620 0.994
τ25/580 580 0.994
τ25/546 546 0.994
τ25/500 500 0.986
τ25/460 460 0.968
τ25/436 436 0.930
τ25/420 420 0.860
τ25/405 405 0.730
τ25/400 400 0.660
τ25/390 390 0.450
τ25/380 380 0.198
τ25/370 370 0.010
τ25/365 365
τ25/350 350
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.891
τ10/2325 2,325 0.910
τ10/1970 1,970 0.971
τ10/1530 1,530 0.996
τ10/1060 1,060 0.999
τ10/700 700 0.998
τ10/660 660 0.998
τ10/620 620 0.998
τ10/580 580 0.998
τ10/546 546 0.998
τ10/500 500 0.994
τ10/460 460 0.987
τ10/436 436 0.971
τ10/420 420 0.941
τ10/405 405 0.882
τ10/400 400 0.847
τ10/390 390 0.727
τ10/380 380 0.523
τ10/370 370 0.160
τ10/365 365 0.040
τ10/350 350
τ10/334 334
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.1976
PC,s 0.4539
Pd,C 0.2859
Pe,d 0.2356
Pg,F 0.6160
Pi,h
P's,t 0.1942
P'C',s 0.4895
P'd,C' 0.2373
P'e,d 0.2315
P'g,F' 0.5443
P'i,h
Characteristics
ΔPC,t -0.0065
ΔPC,s -0.0046
ΔPF,e 0.0026
ΔPg,F 0.0123
ΔPi,g