SF5

Glass Code:  673322.407

A classic glass type with lead oxide as an essential component for outstanding optical properties.

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.67270 νd 32.21
ne 1.67764 νe 31.97
nF-nC 0.020885 nF'-nC' 0.021195
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.63289
n1,970.1 1,970.1 1.63785
n1,529.6 1,529.6 1.64359
n1,060.0 1,060.0 1.65104
nt 1,014.0 1.65206
ns 852.1 1.65664
nr 706.5 1.66327
nC 656.3 1.66661
nC' 643.8 1.66756
Characteristics λ [nm]
n632.8 632.8 1.66846
nD 589.3 1.67252
nd 587.6 1.67270
ne 546.1 1.67764
nF 486.1 1.68750
nF' 480.0 1.68876
ng 435.8 1.69986
nh 404.7 1.71069
ni 365.0 1.73056
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.660
τ25/2325 2,325 0.740
τ25/1970 1,970 0.900
τ25/1530 1,530 0.987
τ25/1060 1,060 0.996
τ25/700 700 0.996
τ25/660 660 0.995
τ25/620 620 0.995
τ25/580 580 0.996
τ25/546 546 0.996
τ25/500 500 0.993
τ25/460 460 0.988
τ25/436 436 0.982
τ25/420 420 0.973
τ25/405 405 0.959
τ25/400 400 0.950
τ25/390 390 0.920
τ25/380 380 0.880
τ25/370 370 0.800
τ25/365 365 0.730
τ25/350 350 0.310
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.847
τ10/2325 2,325 0.887
τ10/1970 1,970 0.959
τ10/1530 1,530 0.995
τ10/1060 1,060 0.998
τ10/700 700 0.998
τ10/660 660 0.998
τ10/620 620 0.998
τ10/580 580 0.998
τ10/546 546 0.998
τ10/500 500 0.997
τ10/460 460 0.995
τ10/436 436 0.993
τ10/420 420 0.989
τ10/405 405 0.983
τ10/400 400 0.980
τ10/390 390 0.967
τ10/380 380 0.950
τ10/370 370 0.915
τ10/365 365 0.882
τ10/350 350 0.626
τ10/334 334 0.200
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2194
PC,s 0.4775
Pd,C 0.2915
Pe,d 0.2366
Pg,F 0.5919
Pi,h 0.9513
P's,t 0.2162
P'C',s 0.5153
P'd,C' 0.2423
P'e,d 0.2331
P'g,F' 0.5237
P'i,h 0.9374
Characteristics
ΔPC,t -0.0010
ΔPC,s -0.0005
ΔPF,e 0.0005
ΔPg,F 0.0023
ΔPi,g 0.0160