Glass Code:  785258.474

A classic glass type with lead oxide as an essential component for outstanding optical properties.

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.78472 νd 25.76
ne 1.79190 νe 25.55
nF-nC 0.030467 nF'-nC' 0.030997
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.73294
n1,970.1 1,970.1 1.73843
n1,529.6 1,529.6 1.74506
n1,060.0 1,060.0 1.75445
nt 1,014.0 1.75579
ns 852.1 1.76200
nr 706.5 1.77125
nC 656.3 1.77599
nC' 643.8 1.77734
Characteristics λ [nm]
n632.8 632.8 1.77862
nD 589.3 1.78446
nd 587.6 1.78472
ne 546.1 1.79190
nF 486.1 1.80645
nF' 480.0 1.80834
ng 435.8 1.82518
nh 404.7 1.84208
ni 365.0
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.610
τ25/2325 2,325 0.700
τ25/1970 1,970 0.930
τ25/1530 1,530 0.982
τ25/1060 1,060 0.997
τ25/700 700 0.993
τ25/660 660 0.991
τ25/620 620 0.991
τ25/580 580 0.991
τ25/546 546 0.989
τ25/500 500 0.976
τ25/460 460 0.940
τ25/436 436 0.860
τ25/420 420 0.700
τ25/405 405 0.340
τ25/400 400 0.200
τ25/390 390 0.010
τ25/380 380
τ25/370 370
τ25/365 365
τ25/350 350
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.821
τ10/2325 2,325 0.867
τ10/1970 1,970 0.971
τ10/1530 1,530 0.993
τ10/1060 1,060 0.999
τ10/700 700 0.997
τ10/660 660 0.996
τ10/620 620 0.996
τ10/580 580 0.996
τ10/546 546 0.996
τ10/500 500 0.990
τ10/460 460 0.976
τ10/436 436 0.941
τ10/420 420 0.867
τ10/405 405 0.650
τ10/400 400 0.525
τ10/390 390 0.180
τ10/380 380
τ10/370 370
τ10/365 365
τ10/350 350
τ10/334 334
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2039
PC,s 0.4590
Pd,C 0.2866
Pe,d 0.2356
Pg,F 0.6147
Pi,h
P's,t 0.2004
P'C',s 0.4949
P'd,C' 0.2380
P'e,d 0.2316
P'g,F' 0.5433
P'i,h
Characteristics
ΔPC,t -0.0043
ΔPC,s -0.0040
ΔPF,e 0.0029
ΔPg,F 0.0142
ΔPi,g