Please be advised that there may be delays in processing new registrations between December 23, 2025, and January 5, 2026.
We appreciate your understanding and cooperation during this period and wish you a joyful holiday season and a successful New Year 2026.
Thank you for your continued trust in our services.

P-SF8

Glass Code:  689313.290

"P" glass suitable for precision molding (low-Tg-glass).

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.68893 νd 31.25
ne 1.69414 νe 31.01
nF-nC 0.022046 nF'-nC' 0.022386
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.64480
n1,970.1 1,970.1 1.65079
n1,529.6 1,529.6 1.65760
n1,060.0 1,060.0 1.66598
nt 1,014.0 1.66708
ns 852.1 1.67200
nr 706.5 1.67901
nC 656.3 1.68252
nC' 643.8 1.68353
Characteristics λ [nm]
n632.8 632.8 1.68447
nD 589.3 1.68874
nd 587.6 1.68893
ne 546.1 1.69414
nF 486.1 1.70457
nF' 480.0 1.70591
ng 435.8 1.71778
nh 404.7 1.72950
ni 365.0
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.450
τ25/2325 2,325 0.570
τ25/1970 1,970 0.850
τ25/1530 1,530 0.977
τ25/1060 1,060 0.997
τ25/700 700 0.988
τ25/660 660 0.984
τ25/620 620 0.984
τ25/580 580 0.987
τ25/546 546 0.986
τ25/500 500 0.972
τ25/460 460 0.950
τ25/436 436 0.930
τ25/420 420 0.900
τ25/405 405 0.850
τ25/400 400 0.820
τ25/390 390 0.710
τ25/380 380 0.480
τ25/370 370 0.150
τ25/365 365 0.040
τ25/350 350
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.727
τ10/2325 2,325 0.799
τ10/1970 1,970 0.937
τ10/1530 1,530 0.991
τ10/1060 1,060 0.999
τ10/700 700 0.995
τ10/660 660 0.994
τ10/620 620 0.994
τ10/580 580 0.995
τ10/546 546 0.994
τ10/500 500 0.989
τ10/460 460 0.980
τ10/436 436 0.971
τ10/420 420 0.959
τ10/405 405 0.937
τ10/400 400 0.924
τ10/390 390 0.872
τ10/380 380 0.746
τ10/370 370 0.468
τ10/365 365 0.260
τ10/350 350 0.001
τ10/334 334
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2229
PC,s 0.4776
Pd,C 0.2905
Pe,d 0.2362
Pg,F 0.5991
Pi,h
P's,t 0.2195
P'C',s 0.5150
P'd,C' 0.2414
P'e,d 0.2326
P'g,F' 0.5301
P'i,h
Characteristics
ΔPC,t 0.0072
ΔPC,s 0.0018
ΔPF,e 0.0013
ΔPg,F 0.0079
ΔPi,g