N-SSK2

Glass Code:  622533.353

“N”-glass as an environmentally friendly alternative to conventional lead and arsenic-containing glass types.

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.62229 νd 53.27
ne 1.62508 νe 52.99
nF-nC 0.011681 nF'-nC' 0.011795
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.59149
n1,970.1 1,970.1 1.59685
n1,529.6 1,529.6 1.60260
n1,060.0 1,060.0 1.60880
nt 1,014.0 1.60953
ns 852.1 1.61264
nr 706.5 1.61678
nC 656.3 1.61877
nC' 643.8 1.61933
Characteristics λ [nm]
n632.8 632.8 1.61985
nD 589.3 1.62219
nd 587.6 1.62229
ne 546.1 1.62508
nF 486.1 1.63045
nF' 480.0 1.63112
ng 435.8 1.63691
nh 404.7 1.64232
ni 365.0 1.65166
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.500
τ25/2325 2,325 0.720
τ25/1970 1,970 0.930
τ25/1530 1,530 0.981
τ25/1060 1,060 0.992
τ25/700 700 0.996
τ25/660 660 0.994
τ25/620 620 0.993
τ25/580 580 0.995
τ25/546 546 0.995
τ25/500 500 0.992
τ25/460 460 0.985
τ25/436 436 0.980
τ25/420 420 0.975
τ25/405 405 0.963
τ25/400 400 0.954
τ25/390 390 0.920
τ25/380 380 0.860
τ25/370 370 0.750
τ25/365 365 0.670
τ25/350 350 0.250
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.758
τ10/2325 2,325 0.877
τ10/1970 1,970 0.971
τ10/1530 1,530 0.992
τ10/1060 1,060 0.997
τ10/700 700 0.998
τ10/660 660 0.998
τ10/620 620 0.997
τ10/580 580 0.998
τ10/546 546 0.998
τ10/500 500 0.997
τ10/460 460 0.994
τ10/436 436 0.992
τ10/420 420 0.990
τ10/405 405 0.985
τ10/400 400 0.981
τ10/390 390 0.967
τ10/380 380 0.941
τ10/370 370 0.891
τ10/365 365 0.852
τ10/350 350 0.574
τ10/334 334 0.084
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2661
PC,s 0.5246
Pd,C 0.3016
Pe,d 0.2381
Pg,F 0.5526
Pi,h 0.7997
P's,t 0.2636
P'C',s 0.5669
P'd,C' 0.2513
P'e,d 0.2358
P'g,F' 0.4902
P'i,h 0.7920
Characteristics
ΔPC,t -0.0069
ΔPC,s -0.0025
ΔPF,e -0.0001
ΔPg,F -0.0016
ΔPi,g -0.0146