N-BAF10

Glass Code:  670471.375

“N”-glass as an environmentally friendly alternative to conventional lead and arsenic-containing glass types.

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.67003 νd 47.11
ne 1.67341 νe 46.83
nF-nC 0.014222 nF'-nC' 0.014380
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.63524
n1,970.1 1,970.1 1.64094
n1,529.6 1,529.6 1.64714
n1,060.0 1,060.0 1.65404
nt 1,014.0 1.65488
ns 852.1 1.65849
nr 706.5 1.66339
nC 656.3 1.66578
nC' 643.8 1.66645
Characteristics λ [nm]
n632.8 632.8 1.66708
nD 589.3 1.66990
nd 587.6 1.67003
ne 546.1 1.67341
nF 486.1 1.68000
nF' 480.0 1.68083
ng 435.8 1.68801
nh 404.7 1.69480
ni 365.0
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.450
τ25/2325 2,325 0.680
τ25/1970 1,970 0.920
τ25/1530 1,530 0.980
τ25/1060 1,060 0.994
τ25/700 700 0.994
τ25/660 660 0.990
τ25/620 620 0.991
τ25/580 580 0.990
τ25/546 546 0.990
τ25/500 500 0.981
τ25/460 460 0.967
τ25/436 436 0.954
τ25/420 420 0.940
τ25/405 405 0.900
τ25/400 400 0.880
τ25/390 390 0.800
τ25/380 380 0.660
τ25/370 370 0.440
τ25/365 365 0.310
τ25/350 350 0.010
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.727
τ10/2325 2,325 0.857
τ10/1970 1,970 0.967
τ10/1530 1,530 0.992
τ10/1060 1,060 0.998
τ10/700 700 0.998
τ10/660 660 0.996
τ10/620 620 0.996
τ10/580 580 0.996
τ10/546 546 0.996
τ10/500 500 0.992
τ10/460 460 0.987
τ10/436 436 0.981
τ10/420 420 0.976
τ10/405 405 0.959
τ10/400 400 0.950
τ10/390 390 0.915
τ10/380 380 0.847
τ10/370 370 0.720
τ10/365 365 0.626
τ10/350 350 0.176
τ10/334 334
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2539
PC,s 0.5122
Pd,C 0.2989
Pe,d 0.2377
Pg,F 0.5629
Pi,h
P's,t 0.2511
P'C',s 0.5533
P'd,C' 0.2489
P'e,d 0.2351
P'g,F' 0.4990
P'i,h
Characteristics
ΔPC,t -0.0024
ΔPC,s -0.0005
ΔPF,e -0.0003
ΔPg,F -0.0016
ΔPi,g