LASF35

Glass Code:  022291.541
optical glass klein 4zu3.jpg
Characteristics
nd 2.02204 νd 29.06
ne 2.03035 νe 28.84
nF-nC 0.035170 nF'-nC' 0.035721
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.95946
n1,970.1 1,970.1 1.96639
n1,529.6 1,529.6 1.97472
n1,060.0 1,060.0 1.98624
nt 1,014.0 1.98786
ns 852.1 1.99531
nr 706.5 2.00628
nC 656.3 2.01185
nC' 643.8 2.01343
Characteristics λ [nm]
n632.8 632.8 2.01493
nD 589.3 2.02173
nd 587.6 2.02204
ne 546.1 2.03035
nF 486.1 2.04702
nF' 480.0 2.04916
ng 435.8 2.06805
nh 404.7 2.08663
ni 365.0
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.550
τ25/2325 2,325 0.720
τ25/1970 1,970 0.934
τ25/1530 1,530 0.987
τ25/1060 1,060 0.994
τ25/700 700 0.981
τ25/660 660 0.974
τ25/620 620 0.969
τ25/580 580 0.962
τ25/546 546 0.943
τ25/500 500 0.874
τ25/460 460 0.774
τ25/436 436 0.670
τ25/420 420 0.550
τ25/405 405 0.390
τ25/400 400 0.320
τ25/390 390 0.180
τ25/380 380 0.050
τ25/370 370 0.000
τ25/365 365
τ25/350 350
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.787
τ10/2325 2,325 0.877
τ10/1970 1,970 0.973
τ10/1530 1,530 0.995
τ10/1060 1,060 0.998
τ10/700 700 0.992
τ10/660 660 0.990
τ10/620 620 0.987
τ10/580 580 0.985
τ10/546 546 0.977
τ10/500 500 0.948
τ10/460 460 0.903
τ10/436 436 0.852
τ10/420 420 0.787
τ10/405 405 0.686
τ10/400 400 0.634
τ10/390 390 0.504
τ10/380 380 0.302
τ10/370 370 0.100
τ10/365 365 0.030
τ10/350 350 0.000
τ10/334 334
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2118
PC,s 0.4701
Pd,C 0.2899
Pe,d 0.2364
Pg,F 0.5982
Pi,h
P's,t 0.2086
P'C',s 0.5073
P'd,C' 0.2409
P'e,d 0.2327
P'g,F' 0.5291
P'i,h
Characteristics
ΔPC,t -0.0009
ΔPC,s -0.0006
ΔPF,e 0.0006
ΔPg,F 0.0033
ΔPi,g