Technical Details
        
            Refractive Indices
        
| Characteristics | λ [nm] | |
|---|---|---|
| n2,325.4 | 2,325.4 | 1.70211 | 
| n1,970.1 | 1,970.1 | 1.70934 | 
| n1,529.6 | 1,529.6 | 1.71726 | 
| n1,060.0 | 1,060.0 | 1.72642 | 
| nt | 1,014.0 | 1.72758 | 
| ns | 852.1 | 1.73264 | 
| nr | 706.5 | 1.73970 | 
| nC | 656.3 | 1.74319 | 
| nC' | 643.8 | 1.74418 | 
| Characteristics | λ [nm] | |
|---|---|---|
| n632.8 | 632.8 | 1.74511 | 
| nD | 589.3 | 1.74931 | 
| nd | 587.6 | 1.74950 | 
| ne | 546.1 | 1.75458 | 
| nF | 486.1 | 1.76464 | 
| nF' | 480.0 | 1.76592 | 
| ng | 435.8 | 1.77713 | 
| nh | 404.7 | 1.78798 | 
| ni | 365.0 | 1.80762 | 
| Characteristics | λ [nm] | |
|---|---|---|
| n334.1 | 334.1 | |
| n312.6 | 312.6 | |
| n296.7 | 296.7 | |
| n280.4 | 280.4 | |
| n248.3 | 248.3 | |
        
            Internal Transmittance
        
| Characteristics | λ [nm] | |
|---|---|---|
| τ25/2500 | 2,500 | 0.090 | 
| τ25/2325 | 2,325 | 0.410 | 
| τ25/1970 | 1,970 | 0.850 | 
| τ25/1530 | 1,530 | 0.960 | 
| τ25/1060 | 1,060 | 0.996 | 
| τ25/700 | 700 | 0.996 | 
| τ25/660 | 660 | 0.995 | 
| τ25/620 | 620 | 0.995 | 
| τ25/580 | 580 | 0.995 | 
| τ25/546 | 546 | 0.994 | 
| τ25/500 | 500 | 0.994 | 
| τ25/460 | 460 | 0.982 | 
| τ25/436 | 436 | 0.965 | 
| τ25/420 | 420 | 0.940 | 
| τ25/405 | 405 | 0.880 | 
| τ25/400 | 400 | 0.850 | 
| τ25/390 | 390 | 0.780 | 
| τ25/380 | 380 | 0.650 | 
| τ25/370 | 370 | 0.400 | 
| τ25/365 | 365 | 0.220 | 
| τ25/350 | 350 | 0.010 | 
| τ25/334 | 334 | |
| τ25/320 | 320 | |
| τ25/310 | 310 | |
| τ25/300 | 300 | |
| τ25/290 | 290 | |
| τ25/280 | 280 | |
| τ25/270 | 270 | |
| τ25/260 | 260 | |
| τ25/250 | 250 | |
| Characteristics | λ [nm] | |
|---|---|---|
| τ10/2500 | 2,500 | 0.382 | 
| τ10/2325 | 2,325 | 0.700 | 
| τ10/1970 | 1,970 | 0.937 | 
| τ10/1530 | 1,530 | 0.984 | 
| τ10/1060 | 1,060 | 0.998 | 
| τ10/700 | 700 | 0.998 | 
| τ10/660 | 660 | 0.998 | 
| τ10/620 | 620 | 0.998 | 
| τ10/580 | 580 | 0.998 | 
| τ10/546 | 546 | 0.998 | 
| τ10/500 | 500 | 0.998 | 
| τ10/460 | 460 | 0.993 | 
| τ10/436 | 436 | 0.986 | 
| τ10/420 | 420 | 0.976 | 
| τ10/405 | 405 | 0.950 | 
| τ10/400 | 400 | 0.937 | 
| τ10/390 | 390 | 0.905 | 
| τ10/380 | 380 | 0.842 | 
| τ10/370 | 370 | 0.693 | 
| τ10/365 | 365 | 0.546 | 
| τ10/350 | 350 | 0.125 | 
| τ10/334 | 334 | |
| τ10/320 | 320 | |
| τ10/310 | 310 | |
| τ10/300 | 300 | |
| τ10/290 | 290 | |
| τ10/280 | 280 | |
| τ10/270 | 270 | |
| τ10/260 | 260 | |
| τ10/250 | 250 | |
        
            Partial Dispersion
        
| Characteristics | |
|---|---|
| Ps,t | 0.2360 | 
| PC,s | 0.4921 | 
| Pd,C | 0.2941 | 
| Pe,d | 0.2369 | 
| Pg,F | 0.5825 | 
| Pi,h | 0.9160 | 
| P's,t | 0.2329 | 
| P'C',s | 0.5311 | 
| P'd,C' | 0.2446 | 
| P'e,d | 0.2338 | 
| P'g,F' | 0.5158 | 
| P'i,h | 0.9037 | 
| Characteristics | |
|---|---|
| ΔPC,t | 0.0174 | 
| ΔPC,s | 0.0078 | 
| ΔPF,e | -0.0011 | 
| ΔPg,F | -0.0025 | 
| ΔPi,g | -0.0093 | 
Downloads
Collection Datasheets
Catalog
TIE‘s - Technical Information
                                        TIE-04: Test Report for Delivery Lots of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            230 kB
                                    
                                        TIE-19: Temperature Coefficient of the Refractive Index (EN)
                                    
                                    
                                            PDF 
                                            450 kB
                                    
                                        TIE-25: Striae in Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            1.24 MB
                                    
                                        TIE-26: Homogeneity of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            990 kB
                                    
                                        TIE-27: Stress in Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            710 kB
                                    
                                        TIE-28: Bubbles and Inclusions in Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            260 kB
                                    
                                        TIE-30: Chemical Properties of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            210 kB
                                    
                                        TIE-31: Mechanical and Thermal Properties of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            190 kB
                                    
                                        TIE-32: Thermal Loads on Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            100 kB
                                    
                                        TIE-33: Bending Strength of Optical Glass and ZERODUR® (EN)
                                    
                                    
                                            PDF 
                                            2.76 MB
                                    
                                        TIE-35: Transmittance of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            510 kB
                                    
                                        TIE-36: Fluorescence of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            710 kB
                                    
                                        TIE-40: Optical Glass for Precision Molding (EN)
                                    
                                    
                                            PDF 
                                            610 kB
                                    
                                        TIE-41: Large Optical Glass Blanks (EN)
                                    
                                    
                                            PDF 
                                            2.06 MB