F5

Glass Code:  603380.347

A classic glass type with lead oxide as an essential component for outstanding optical properties.

Find more information in the tabs below or on our website.

Compare glass types with our Interactive Abbe Diagram.

optical glass klein 4zu3.jpg
Characteristics
nd 1.60342 νd 38.03
ne 1.60718 νe 37.77
nF-nC 0.015867 nF'-nC' 0.016078
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
DIA
Step
nd
Step
vd
nd
vd
Weight
 
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.56934
n1,970.1 1,970.1 1.57427
n1,529.6 1,529.6 1.57979
n1,060.0 1,060.0 1.58636
nt 1,014.0 1.58721
ns 852.1 1.59093
nr 706.5 1.59616
nC 656.3 1.59875
nC' 643.8 1.59948
Characteristics λ [nm]
n632.8 632.8 1.60017
nD 589.3 1.60328
nd 587.6 1.60342
ne 546.1 1.60718
nF 486.1 1.61461
nF' 480.0 1.61556
ng 435.8 1.62381
nh 404.7 1.63176
ni 365.0 1.64606
Characteristics λ [nm]
n334.1 334.1 1.66276
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.550
τ25/2325 2,325 0.650
τ25/1970 1,970 0.860
τ25/1530 1,530 0.987
τ25/1060 1,060 0.998
τ25/700 700 0.997
τ25/660 660 0.996
τ25/620 620 0.995
τ25/580 580 0.995
τ25/546 546 0.995
τ25/500 500 0.994
τ25/460 460 0.991
τ25/436 436 0.990
τ25/420 420 0.988
τ25/405 405 0.985
τ25/400 400 0.982
τ25/390 390 0.973
τ25/380 380 0.960
τ25/370 370 0.930
τ25/365 365 0.910
τ25/350 350 0.760
τ25/334 334 0.300
τ25/320 320 0.000
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.787
τ10/2325 2,325 0.842
τ10/1970 1,970 0.941
τ10/1530 1,530 0.995
τ10/1060 1,060 0.999
τ10/700 700 0.999
τ10/660 660 0.998
τ10/620 620 0.998
τ10/580 580 0.998
τ10/546 546 0.998
τ10/500 500 0.998
τ10/460 460 0.996
τ10/436 436 0.996
τ10/420 420 0.995
τ10/405 405 0.994
τ10/400 400 0.993
τ10/390 390 0.989
τ10/380 380 0.984
τ10/370 370 0.971
τ10/365 365 0.963
τ10/350 350 0.896
τ10/334 334 0.618
τ10/320 320 0.080
τ10/310 310 0.000
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2346
PC,s 0.4925
Pd,C 0.2946
Pe,d 0.2371
Pg,F 0.5795
Pi,h 0.9015
P's,t 0.2315
P'C',s 0.5317
P'd,C' 0.2451
P'e,d 0.2340
P'g,F' 0.5131
P'i,h 0.8897
Characteristics
ΔPC,t 0.0017
ΔPC,s 0.0009
ΔPF,e -0.0001
ΔPg,F -0.0003
ΔPi,g -0.0028