| Propriétés mécaniques |   | 
        ||||||
|---|---|---|---|---|---|---|---|
| Density p (annealed at 40 °C/h)  | 
            2.46 g/cm3 | 
        ||||||
| Chemical strengthening | thickness in mm temperature J in °C time t in min compressive stress (CS) in MPa depth of layer (DoL) in μm  | 
            
             0.075 > 10  | 
            
             0.33 > 12  | 
        ||||
| Young‘s modulus E | 71.9 kN/mm2 | ||||||
| Poisson‘s ratio μ | 0.216 | ||||||
| Torsion modulus G | 29.6 kN/mm2 | ||||||
| Knoop hardness HK 0.1/20 | 490 | ||||||
| Vickers hardness HV 0.2/25 | 560 | ||||||
| Propriétés thermiques | |||||||
|---|---|---|---|---|---|---|---|
| Coefficient of thermal expansion (CTE) α (20-300 °C)  | 
            9.2 · 10-6 K-1 | 
        ||||||
| Mean specific heat capacity c p(20 –100 °C)  | 
            0.87 J/(g · K) | 
        ||||||
| Transformation temperature Tg | 598 °C | ||||||
| Viscosities | Viscosity  in η in dPas  | 
            Temperature in °C  | 
        |||||
| Strain point | 14.5 | 577 | |||||
| Annealing point | 13.0 | 616 | |||||
| Softening point | 7.6 | 855 | |||||
| Propriétés optiques | |||||||
|---|---|---|---|---|---|---|---|
| Refractive indices | ng | 1.5151 | |||||
| Pretreatment of samples | nF' | 1.5109 | |||||
| Condition as supplied | nF | 1.5104 | |||||
| [„as drawn“] | ne | 1.5065 | |||||
| nd | 1.5044 | ||||||
| nD | 1.5043 ± 0.0015 | ||||||
| nC' | 1.5022 | ||||||
| nC | 1.5017 | ||||||
| Abbe value | ve | 57.7 | |||||
| Photoelastic constant C  [nm/(cm*MPa)]  | 
            29.0 | ||||||
| Transmittance values | |||||||
|---|---|---|---|---|---|---|---|
| Thickness 0.33 mm | wavelength at 254 nm at 380 nm at 632.8 nm at 1064 nm  | 
            τ (λ) in % 31.1 91.6 92.2 92.4  | 
        |||||
| Edge wavelength λC ( τ = 0.46)  | 
            thickness in mm 0.075 0.33  | 
            wavelength in nm 230 266  | 
        |||||
| Luminous transmittance τvD65 in %  | 
            0.33 | 92 | |||||
| Propriétés chimiques | ||||||||
|---|---|---|---|---|---|---|---|---|
| Hydrolytic resistance acc. to DIN ISO 719 | ||||||||
| Class | HGB 2 | 
        |||||||
| Equivalent of alkali per gram of glass grains [µg/g] | 56 | |||||||
| Acid resistance acc. to DIN 12 116 | ||||||||
| Class | S 4 | |||||||
| Half surface weight loss after 6 hours [mg/dm²] | 61 | |||||||
| Alkali resistance acc. to ISO 695 | ||||||||
| Class | A 1 | |||||||
| Surface weight loss after 3 hours [mg/dm²] | 66 | |||||||
| Propriétés électriques | |||||||
|---|---|---|---|---|---|---|---|
| Dielectric constant ɛr (at ν = 25°C)  | 
            at 1 MHz at 1 GHz at 5 GHz  | 
            8.4 7.6 7.5  | 
        |||||
| Dissipation factor tan δ (at ν = 25°C)  | 
            at 1 MHz at 1 GHz at 5 GHz  | 
            252 · 10-4 176 · 10-4 217 · 10-4  | 
        |||||
| Conductivity (at ν = 25°C)  | 
            in S/cm direct current  | 
            160 · 10-12 | |||||