Technical Details of Xensation®
Technical excellence for maximum cover glass protection and durability
Mechanical properties
| Description | Xensation® Core | Xensation® α | Xensation® Up. |
|---|---|---|---|
| Density ρ | 2.38 g/cm3 | 2.39 g/cm3 | 2.48 g/cm3 |
| Young’s modulus E | 78 kN/mm2 | 80 kN/mm2 | 82 kN/mm2 |
| Poisson’s ratio ν | 0.22 | 0.26 | 0.22 |
| Shear modulus G | 32 kN/mm2 | 32 kN/mm2 | 34 kN/mm2 |
| Vickers hardness HV | |||
| > unstrengthened | 610 | 570 | 630 |
| > strengthened* | 670 | 660 | 680 |
All values are typical measured values and refer to unstrengthended glass
Thermal properties
| Description | Xensation® Core | Xensation® α | Xensation® Up. |
|---|---|---|---|
| Coefficient of mean linear thermal expansion α(20 – 300 °C) | 5.0 · 10-6 K-1 | 5.3 · 10 –6 K–1 | 8.3 · 10 –6 K–1 |
| Transformation temperature Tg | 580 °C | 577 °C | 525 °C |
| Viscosity | |||
| > Annealing point at 1013 dPas | 590 °C | 589 °C | 540 °C |
| > Softening point at 107.6 dPas | 820 °C | 840 °C | 760 °C |
| > Working point at 104 dPas | 1190 °C | 1233 °C | 1120 °C |
All values are typical measured values and refer to unstrengthended glass
Optical properties
| Description | Xensation® Core | Xensation® α | Xensation® Up. |
|---|---|---|---|
| Wavelength λ [nm] | 595 nm |
||
| Measurement method | FSM-LE | ||
| Refractive index n of core glass | 1.511 | 1.508 | 1.521 |
| Photoelastic constant C [nm/(cm*MPa)] | 31.0 | 30.0 | 27.8 |
| Transmittance T [%] (t = 0.78 mm) | >91 | >91 | >91 |
All values are typical measured values and refer to unstrengthended glass
Chemical properties
| Description | Xensation® Core | Xensation® α | Xensation® Up. |
|---|---|---|---|
| Hydrolytic resistance acc. to DIN ISO 719 | |||
| > Hydrolytic class | HGB 1 | HGB1 | HGB2 |
| > Equivalent of alkali Na2O per gram of glass grains [µg/g] | 21 | 32 | 38 |
| Acid resistance acc. to DIN 12 116 | |||
| > Acid class | S3 | S2 | S4 |
| > Half surface weight loss after 6 hours [mg/dm²] | 8.5 | 1.4 | 19 |
| Alkali resistance acc. to DIN ISO 695 | |||
| > Alkali class | A2 | A2 | A1 |
| > Surface weight loss after 3 hours [mg/dm²] | 104 | 92 | 42 |
All values are typical measured values and refer to unstrengthended glass
Electrical properties (extrapolated)
| Xensation® Core | Xensation® α | Xensation® Up. | ||||
|---|---|---|---|---|---|---|
| Frequency ƒ0 [MHz] | Dielectric constant ε | Loss tangent tan δ | Dielectric constant ε | Loss tangent tan δ | Dielectric constant ε | Loss tangent tan δ |
| 54 | 6.1 | 0.009 | 6.1 | 0.008 | 7.3 | 0.007 |
| 480 | 6.0 | 0.010 | 6.0 | 0.009 | 7.1 | 0.008 |
| 825 | 6.0 | 0.010 | 6.0 | 0.010 | 7.1 | 0.009 |
| 912 | 6.0 | 0.010 | 6.0 | 0.010 | 7.1 | 0.009 |
| 1977 | 6.0 | 0.011 | 6.0 | 0.011 | 7.0 | 0.010 |
| 2170 | 6.0 | 0.011 | 6.0 | 0.011 | 7.0 | 0.010 |
| 2986 | 5.9 | 0.011 | 6.0 | 0.012 | 7.0 | 0.011 |
All values are typical measured values and refer to unstrengthended glass
Chemical strengthening*
| Description | Xensation® Core | Xensation® α | Xensation® Up. |
|---|---|---|---|
| Compressive stress CS | capable > 900 MPa | capable > 900 MPa | capable > 900 MPa |
| Depth of compressive layer DoCL | capable >180 μm | capable > 180 µm | capable > 150 µm |
| 4-Point bending strength | capable > 800 MPa | capable > 800 MPa | capable > 700 MPa |
* Values that can be achieved after chemical strengthening process
Forms supplied**
| Description | Xensation® Core | Xensation® α | Xensation® Up. |
|---|---|---|---|
| Thickness range | 0.50 - 0.70 mm | 0.55 – 0.80 mm | 0.55 – 0.80 mm |
| Sheet size | 1150 mm x 950 mm | 1150 mm x 950 mm | 1150 mm x 950 mm |
** Further thicknesses and sheet sizes are available on request