Technical Details of Xensation®
Technical excellence for maximum cover glass protection and durability
Mechanical properties
Description | Xensation® Core | Xensation® α | Xensation® Up. |
---|---|---|---|
Density ρ | 2.38 g/cm3 | 2.39 g/cm3 | 2.48 g/cm3 |
Young’s modulus E | 78 kN/mm2 | 80 kN/mm2 | 82 kN/mm2 |
Poisson’s ratio ν | 0.22 | 0.26 | 0.22 |
Shear modulus G | 32 kN/mm2 | 32 kN/mm2 | 34 kN/mm2 |
Vickers hardness HV | |||
> unstrengthened | 610 | 570 | 630 |
> strengthened* | 670 | 660 | 680 |
All values are typical measured values and refer to unstrengthended glass
Thermal properties
Description | Xensation® Core | Xensation® α | Xensation® Up. |
---|---|---|---|
Coefficient of mean linear thermal expansion α(20 – 300 °C) | 5.0 · 10-6 K-1 | 5.3 · 10 –6 K–1 | 8.3 · 10 –6 K–1 |
Transformation temperature Tg | 580 °C | 577 °C | 525 °C |
Viscosity | |||
> Annealing point at 1013 dPas | 590 °C | 589 °C | 540 °C |
> Softening point at 107.6 dPas | 820 °C | 840 °C | 760 °C |
> Working point at 104 dPas | 1190 °C | 1233 °C | 1120 °C |
All values are typical measured values and refer to unstrengthended glass
Optical properties
Description | Xensation® Core | Xensation® α | Xensation® Up. |
---|---|---|---|
Wavelength λ [nm] | 595 nm |
||
Measurement method | FSM-LE | ||
Refractive index n of core glass | 1.511 | 1.508 | 1.521 |
Photoelastic constant C [nm/(cm*MPa)] | 31.0 | 30.0 | 27.8 |
Transmittance T [%] (t = 0.78 mm) | >91 | >91 | >91 |
All values are typical measured values and refer to unstrengthended glass
Chemical properties
Description | Xensation® Core | Xensation® α | Xensation® Up. |
---|---|---|---|
Hydrolytic resistance acc. to DIN ISO 719 | |||
> Hydrolytic class | HGB 1 | HGB1 | HGB2 |
> Equivalent of alkali Na2O per gram of glass grains [µg/g] | 21 | 32 | 38 |
Acid resistance acc. to DIN 12 116 | |||
> Acid class | S3 | S2 | S4 |
> Half surface weight loss after 6 hours [mg/dm²] | 8.5 | 1.4 | 19 |
Alkali resistance acc. to DIN ISO 695 | |||
> Alkali class | A2 | A2 | A1 |
> Surface weight loss after 3 hours [mg/dm²] | 104 | 92 | 42 |
All values are typical measured values and refer to unstrengthended glass
Electrical properties (extrapolated)
Xensation® Core | Xensation® α | Xensation® Up. | ||||
---|---|---|---|---|---|---|
Frequency ƒ0 [MHz] | Dielectric constant ε | Loss tangent tan δ | Dielectric constant ε | Loss tangent tan δ | Dielectric constant ε | Loss tangent tan δ |
54 | 6.1 | 0.009 | 6.1 | 0.008 | 7.3 | 0.007 |
480 | 6.0 | 0.010 | 6.0 | 0.009 | 7.1 | 0.008 |
825 | 6.0 | 0.010 | 6.0 | 0.010 | 7.1 | 0.009 |
912 | 6.0 | 0.010 | 6.0 | 0.010 | 7.1 | 0.009 |
1977 | 6.0 | 0.011 | 6.0 | 0.011 | 7.0 | 0.010 |
2170 | 6.0 | 0.011 | 6.0 | 0.011 | 7.0 | 0.010 |
2986 | 5.9 | 0.011 | 6.0 | 0.012 | 7.0 | 0.011 |
All values are typical measured values and refer to unstrengthended glass
Chemical strengthening*
Description | Xensation® Core | Xensation® α | Xensation® Up. |
---|---|---|---|
Compressive stress CS | capable > 900 MPa | capable > 900 MPa | capable > 900 MPa |
Depth of compressive layer DoCL | capable >180 μm | capable > 180 µm | capable > 150 µm |
4-Point bending strength | capable > 800 MPa | capable > 800 MPa | capable > 700 MPa |
* Values that can be achieved after chemical strengthening process
Forms supplied**
Description | Xensation® Core | Xensation® α | Xensation® Up. |
---|---|---|---|
Thickness range | 0.50 - 0.70 mm | 0.55 – 0.80 mm | 0.55 – 0.80 mm |
Sheet size | 1150 mm x 950 mm | 1150 mm x 950 mm | 1150 mm x 950 mm |
** Further thicknesses and sheet sizes are available on request