Technical Details of Cut-to-Size Substrates
Technical excellence across the board
Up-drawn cut-to-size substrates
The following specifications are applicable to B 270®:
1. Cutting formats (round, rectangular)
| Thickness in mm | Max. size1 in mm | Min. size1 in mm | Tolerance1 in mm | 
|---|---|---|---|
| 0.9 – 8.0 | 1600 x 800 | 20 x 20 | ± 1.0 | 
| 9.0 – 10.0 | 1600 x 800 | 100 x 100 | ± 2.0 | 
(1) Other sizes or tolerances on request
2. Glass quality properties
Bulk defects
| Quality properties & Specification | ||||
|---|---|---|---|---|
| Bubbles: | length and width ≤ 0.8 mm: allowed | |||
| Area | < 0.1 m² | ≥ 0.1 to < 0.5 m² | ≥ 0.5 to < 1.0 m² | ≥ 1.0 m² | 
| Width | ≤ 0.8 mm | ≤ 0.8 mm | ≤ 0.8 mm | ≤ 0.8 mm | 
| Length | ≤ 5.0 mm | ≤ 8.0 mm | ≤ 10.0 mm | ≤ 10.0 mm | 
| Max. quantity | ≤ 3 pcs. | ≤ 4 pcs. | ≤ 6 pcs. | ≤ 8 pc. | 
| Knots, stones | Ø ≤ 1.5 mm: allowed | |||
| Knot accumulation | not allowed | |||
| Striae | acc. to limit sample | |||
Surface defects
| Quality properties | 
            Specification | 
|---|---|
| Scratches | see specification for bubbles above | 
| Hair scratches | length ≤ 30 mm: allowed | 
| Shutter and roller marks | g = (Length+Width)/2 ≤ 1.5 mm: allowed | 
| Open bubbles | see specification for bubbles above | 
| Cullets which stick to the surface | Ø < 1.0 mm: allowed | 
| Drawing stripes | front and backside according to limit sample | 
Edge defects
| Quality properties | Specification | 
|---|---|
| Chipping | ≤ ½ of glass thickness allowed | 
| Cracks | not allowed | 
Defect accumulation 
An accumulation of more then 10 defects, also allowed defects, in an area of 250 x 250 mm is not allowed.  
Down-drawn cut-to-size substrates
The following specifications are applicable to D 263® T eco, D 263® LA eco, AF 32® eco, Solar Glass 0787 and B 270® Thin:
1. Base material formats
| Base material1 | Dimensions | D 263® T eco  in mm  | 
            D 263® LA eco  in mm  | 
            AF 32® eco  in mm  | 
            SCHOTT® Solar Glass 0787  in mm  | 
            B 270® Thin  in mm  | 
        
|---|---|---|---|---|---|---|
| Formats | 
            standard | 510 x 430 | 415 x 360 | 440 x 360 | 560 x 380 | 420 x 340 | 
| Ultra-Thin Glass2 (thickness ≤ 0.1 mm) | max. | 440 x 360 | - | 510 x 430 | 560 x 380 | - | 
| Thickness range | min. | 0.03 | 0.3 | 0.03 | 0.07 | 0.3 | 
| Thickness range | max. | 1.1 | 0.7 | 0.5 | 0.15 | 0.9 | 
(1) Base material is for SCHOTT internal use only
(2) Ultra-Thin Glass is available as sheets only
Special dimensions upon request
2. Geometrical properties
| Thickness1 in mm | Glass Types2 | Thickness Tolerance3  in µm  | 
            Total Thickness  Variation3 (TTV) in µm  | 
            Flatness4  in µm  | 
        
|---|---|---|---|---|
| 0.03 | D 263® T eco | AF 32® eco | ± 10 – 15 | ≤ 15 | ≤ 3000 | 
| 0.05 | D 263® T eco | AF 32® eco | ± 10 – 15 | ≤ 15 | ≤ 3000 | 
| 0.07 | D 263® T eco | AF 32® eco | SCHOTT® Solar Glass 0787 | ± 10 – 15 | ≤ 15 – 30 | ≤ 3000 – 3500 | 
| 0.1 | D 263® T eco | AF 32® eco | SCHOTT® Solar Glass 0787 | ± 10 – 20 | ≤ 10 – 30 | ≤ 1500 – 3500 | 
| 0.125 – 0.150 | SCHOTT® Solar Glass 0787 | ± 15 | ≤ 30 | ≤ 3500 | 
| 0.145 – 0.175 | D 263® T eco | AF 32® eco | ± 10 – 15 | ≤ 10 – 15 | ≤ 1500 | 
| 0.200 – 0.210 | D 263® T eco | AF 32® eco | ± 15 | ≤ 15 | ≤ 200 | 
| 0.25 | D 263® T eco | AF 32® eco | ± 15 | ≤ 15 | ≤ 150 | 
| 0.3 | D 263® T eco | D 263® LA eco | AF 32® eco | B 270® Thin | ± 15 – 20 | ≤ 15 – 20 | ≤ 150 – 400 | 
| 0.4 | D 263® T eco | D 263® LA eco | AF 32® eco | ± 15 – 20 | ≤ 15 – 20 | ≤ 150 – 400 | 
| 0.5 – 0.55 | D 263® T eco | D 263® LA eco | AF 32® eco | ± 15 – 30 | ≤ 15 – 20 | ≤ 150 – 400 | 
| 0.7 | D 263® T eco | D 263® LA eco | ± 15 – 50 | ≤ 15 – 30 | ≤ 250 – 400 | 
| 0.9 | D 263® T eco | B 270® Thin | ± 20 – 25 | ≤ 20- 25 | ≤ 250 | 
| 1.0 | D 263® T eco | ± 20 – 30 | ≤ 20 – 25 | ≤ 250 | 
| 1.1 | D 263® T eco | ± 20 – 50 | ≤ 25 | ≤ 250 | 
(1) other thickness on request 
(2) other glass types on request 
(3) acc. to SEMI MF 1530 GBIR  
(4) acc. to SEMI M1 GBINFER 
3. Cutting formats
| Thickness | Format1 | Maximum size2  in mm  | 
            Minimum size2  in mm  | 
            Tolerance2  in mm  | 
        
|---|---|---|---|---|
| 0.03 mm to ≤ 0.1 mm | rectangular | base material minus 40 mm | 20 x 20 | ± 0.5 | 
| 0.03 mm to ≤ 0.1 mm | round | base material minus 40 mm | Ø 50 | ± 0.5 | 
| ≥ 0.1 mm to ≤ 0.4 mm | rectangular | base material minus 40 mm | 10 x 10 | ± 0.2 | 
| ≥ 0.1 mm to ≤ 0.4 mm | round | base material minus 40 mm | Ø 40 | ± 0.2 | 
| > 0.4 mm to ≤ 1.1 mm | rectangular | base material minus 40 mm | 10 x 10 | ± 0.2 | 
| > 0.4 mm to ≤ 1.1 mm | round | base material minus 40 mm | Ø 40 | ± 0.5 | 
(1) Customized free-form formates on request 
(2) Other sizes and tolerances on request
4. Glass quality properties
| Thickness in mm | Specification | 
|---|---|
| 0.03 - < 0.1 | ≤ 1.0 % (of max. edge) | 
| 0.1 - 1.1 | ≤ 0.5 % (of max. edge) | 
Squareness
| Thickness in mm | Specification | 
|---|---|
| 0.03 - < 0.1 | 
             ≤ 2.0 % (of max. edge)  | 
        
| 0.1 - 1.1 | ≤ 1.0 % (of max. edge) | 
Spot type defects (e.g. inclusions, bubbles, knots, particles, digs)
| Dimension | Specification | 
|---|---|
| Max. edge format or Ø < 100 mm | < 0.1 mm: ignore | 
| ≥ 0.1 mm to ≤ 0.2 mm: ≤ 1 pc. | |
| > 0.2 mm: none | |
| 100 mm to 300 mm | < 0.1 mm: ignore | 
| ≥ 0.1 mm to ≤ 0.2 mm: ≤ 2 pcs. | |
| > 0.2 mm: none | |
| > 300 mm | < 0.1 mm: ignore | 
| ≥ 0.1 mm to ≤ 0.2 mm: ≤ 3 pcs. | |
| > 0.2 mm: none | 
Linear defects (e.g. scratches) | L: length W: width
| Dimension | Specification | 
|---|---|
| Max. edge format or Ø < 100 mm | L ≤ 25 mm and W ≤ 20 µm: ignore | 
| L ≤ 25 mm and W > 20 to 50 µm: ≤ 1 pc. | |
| L > 25 mm or W > 50 µm: none | |
| 100 mm to 300 mm | ≤ 2 defects allowed (as defined for stock sheets) | 
| > 300 mm | ≤ 3 defects allowed (as defined for stock sheets) | 
Edge defects (e.g. chips, protrusions)
| Thickness in mm | Specification | 
|---|---|
| < 0.5 | < 0.1 mm: ignore | 
| < 0.5 mm: ≤ 2 pcs. per edge | |
| > 0.5 mm: none | |
| > 0.5 to < 1.1 | 0.2 mm: ignore | 
| < 1.0 mm: ≤ 2 pcs. per edge | |
| > 1.0 mm: none | 
Cracks
| Condition | Specification | 
|---|---|
| visible | none | 
        
Contaminations
| Condition | Specification | 
|---|---|
| Inspection condition:  light source ≤ 5 klux, dark environment, duration 15s/pc., cleaned  | 
            Contaminations (e.g. glove marks, conveyor belt marks, paper marks, haze, cullet's, dust etc.) can be judged after a suitable cleaning process; cleaning recommendations or technical assistance on cleaning can be provided upon request. Contaminations on un-cleaned glasses will be ignored and are permissible without any size restriction. | 
Quality assurance
| Condition | Specification | 
|---|---|
| AQL according to ISO 2859 | 
            
  | 
        
Floated cut-to-size substrates
The following specifications are applicable to BOROFLOAT®:
| Thickness (mm) | Size min (mm) | Size max (mm) | Tolerances | 
|---|---|---|---|
| 0.4 - 25.4 | 10 x 10 | 1.200 x 1.200 | ± 0.3 to ± 5 mm (higher tolerances for greater thicknesses); greater thicknesses on request  | 
        
| 1.1 - 21.0 | 50 x 50 | 2.200 x 4.200 | 
Cut-to-size substrate materials
The following materials are available as cut-to-size substrates:
- D 263® T eco
 - D 263® LA eco
 - BOROFLOAT®
 - AF 32® eco
 - B 270®
 - Solar Glass 0787
 
To find out more, please see the related materials on the overview page.