Technical Details of D 263®
Outstanding and adaptable technical advantages
Material Properties of D 263® M
1. Optical properties
| Optical Properties | Value | 
|---|---|
| Refractive index* ng | 1.5354 | 
| Refractive index* nF' | 1.5305 | 
| Refractive index* nF | 1.5300 | 
| Refractive index* ne | 1.5255 ± 0.0015 | 
| Refractive index* nd | 1.5231 | 
| Refractive index* nD | 1.5230 | 
| Refractive index* nC' | 1.5209 | 
| Refractive index* nC | 1.5204 | 
| Abbe value νe | 55 | 
| Photoelastic constant in (nm/cm)/Mpa | 34.7 | 
        
* Refractive indices: Pretreatment of samples. 
Condition as supplied ["as drawn"] 
2. Thermal properties
| General thermal properties | Unit | Value | 
|---|---|---|
| CTE (Coefficient of thermal expansion) α | 10-6·K-1 (20 °C; 300 °C) | 7.2 | 
| Mean specific heat capacity cp | in J/(g·K) (20 °C; 100 °C) | 0.8 | 
| Transformation temperature Tg | in °C | 557 | 
        
| Viscosities | Viscosity lg ŋ in dPas | Temperature in °C | 
|---|---|---|
| Strain point | 14.5 | 529 | 
| Annealing point | 13.0 | 557 | 
| Softening point | 7.6 | 736 | 
3. Mechanical properties
| Mechanical Properties | 
            Unit | Value | 
|---|---|---|
| Density ρ | in g/cm³ | 2.51 | 
| Young's modulus E | in kN/mm² | 72.9 | 
| Poisson's ratio µ | 0.21 | |
| Torsion modulus G | in kN/mm² | 30 | 
| Knoop hardness | HK 0.1/20 | 470 | 
| Vickers hardness | HV 0.2/25 | 510 | 
Chemical toughening (for thickness = 0.145 mm)
| Unit | 
            Value | 
|---|---|
| Temperature ϑ in °C | 390 | 
| Time t in h | 4 | 
| Compressive stress (CS) in MPa | 290 | 
| Depth of layer (DoL) in µm | 15 | 
4. Chemical properties
| Hydrolytic resistance (acc. to DIN ISO 719) | Value | 
|---|---|
| Class | HGB 1 | 
| Equivalent of alkali per gram glass grains in µg/g | 20 | 
| Acid resistance (acc. to DIN 12116) | Value | 
|---|---|
| Class | S3 | 
| Half surface weight loss after 6 hours in mg/dm² | 2.1 | 
| Alkali resistance (acc. to DIN ISO 695) | Value | 
|---|---|
| Class | A 2 | 
| Surface weight loss after 3 hours in mg/dm² | 88 | 
5. Electrical properties
| Dielectric constant εr (at ϑ = 25 °C) | Value | 
|---|---|
| at 1 MHz | 6.7 | 
| at 1 GHz | 6.4 | 
| at 5 GHz | 6.3 | 
| Dissipation factor tan δ (at ϑ = 25 °C) | 
            Value | 
|---|---|
| at 1 MHz | 61·10-4 | 
| at 1 GHz | 74·10-4 | 
| at 5 GHz | 101·10-4 | 
| Electric volume resistivity ρD (for alternate current 50 Hz ) | 
        
|---|
| 1.6·108 ( ϑ = 250 °C) | 
| 3.5·106 (ϑ = 350 °C) | 
6. Transmittance values
Spectral transmittance: 250 - 3150 nm

Spectral transmittance: 250 - 450 nm

| Wavelength in nm at thickness 0.145 mm: | τ (λ) in % | 
|---|---|
| 254 | < 0.1 | 
| 380 | 91.2 | 
| 632.8 | 91.9 | 
| 1064 | 92.2 | 
| Edge wavelength λc (τ = 0.46) at thickness in mm | Wavelength in nm | 
|---|---|
| 0.100 | 308 | 
| 0.145 | 312 | 
| 0.175 | 314 | 
| 0.210 | 315 | 
| Luminous transmittance at thickness in mm | τvD65in % | 
|---|---|
| 0.145 | 91.7 ± 0.3 | 
Material properties of D 263® bio
1. Optical properties
| Optical Properties | Value | 
|---|---|
| Refractive index* ng | 1.5354 | 
        
| Refractive index* nF' | 1.5305 | 
        
| Refractive index* nF | 1.5300 | 
| Refractive index* ne | 1.5255 ± 0.0015 | 
| Refractive index* nd | 1.5231 | 
| Refractive index* nD | 1.5230 | 
| Refractive index* nC' | 1.5209 | 
| Refractive index* nC | 1.5204 | 
| Abbe value νe | 55 | 
* Refractive indices: Pretreatment of samples. 
Condition as supplied ["as drawn"] 
2. Thermal properties
| General thermal properties | Unit | Value | 
|---|---|---|
| CTE (Coefficient of thermal expansion) α | 10-6·K-1 (20 °C; 300 °C) | 7.2 | 
| Mean specific heat capacity cp | in J/(g·K)(20 °C; 100 °C) | 0.8 | 
| Transformation temperature Tg | in °C | 557 | 
| Viscosities | Viscosity lg ŋ in dPas | Temperature in °C | 
|---|---|---|
| Strain point | 14.5 | 529 | 
| Annealing point | 13.0 | 557 | 
| Softening point | 7.6 | 736 | 
3. Mechanical properties
| Mechanical Properties | 
            Unit | Value | 
|---|---|---|
| Density ρ | in g/cm³ | 2.51 | 
| Stress optical coefficient C | 1.02·10-12 m²/N | 3.4 | 
| Young's modulus E | in kN/mm² | 72.9 | 
| Poisson's ratio µ | 0.21 | |
| Torsion modulus G | in kN/mm² | 30 | 
| Knoop hardness | HK 0.1/20 | 470 | 
| Vickers hardness | HV 0.2/25 | 510 | 
Chemical toughening (for thickness = 0.3 mm)
| Unit | 
            Value | 
|---|---|
| Temperature ϑ in °C | 410 | 
| Time t in h | 4 | 
| Compressive stress (CS) in MPa | 317 | 
| Depth of layer (DoL) in µm | 18 | 
4. Chemical properties
| Hydrolytic resistance (acc. to DIN ISO 719) | Value | 
|---|---|
| Class | HGB 1 | 
| Equivalent of alkali per gram glass grains in µg/g | 20 | 
| Acid resistance (acc. to DIN 12116) | Value | 
|---|---|
| Class | S 3 | 
| Half surface weight loss after 6 hours in mg/dm² | 2.1 | 
| Alkali resistance (acc. to DIN ISO 695) | Value | 
|---|---|
| Class | A 2 | 
| Surface weight loss after 3 hours in mg/dm² | 88 | 
Auto fluorescence in >80% transmission spectrum

5. Electrical properties
| Dielectric constant εr (at ϑ = 25 °C) | Value | 
|---|---|
| at 1 MHz | 6.7 | 
| at 1 GHz | 6.4 | 
| at 5 GHz | 6.3 | 
| Dissipation factor tan δ (at ϑ = 25 °C) | 
            Value | 
|---|---|
| at 1 MHz | 61·10-4 | 
| at 1 GHz | 74·10-4 | 
| at 5 GHz | 101·10-4 | 
| Electric volume resistivity ρD in Ω·cm alternate current 50 Hz  | 
        
|---|
| 1.6·108 ( ϑ = 250 °C) | 
| 3.5·106 (ϑ = 350 °C) | 
6. Transmittance values
Spectral transmittance: 250 - 3150 nm

Spectral transmittance: 250 - 450 nm

| Wavelength in nm at thickness 0.3 mm: | τ (λ) in % | 
|---|---|
| 254 | < 0.1 | 
| 380 | 91.2 | 
| 632.8 | 92 | 
| 1064 | 92 | 
| Edge wavelength λc (τ = 0.46) at thickness in mm | Wavelength in nm | 
|---|---|
| 0.10 | 
             308  | 
        
| 0.21 | 315 | 
| 0.30 | 318 | 
| 0.40 | 321 | 
| 1.10 | 329 | 
| Luminous transmittance at thickness in mm | τvD65in % | 
|---|---|
| 0.3 | 91.7 ± 0.3 | 
Material properties of D 263®T eco
1. Optical properties
| Optical Properties | Value | 
|---|---|
| Refractive index* ng | 1.5354 | 
        
| Refractive index* nF' | 1.5305 | 
| Refractive index* nF | 1.5300 | 
| Refractive index* ne | 1.5255 ± 0.0015 | 
| Refractive index* nd | 1.5231 | 
| Refractive index* nD | 1.5230 | 
| Refractive index* nC' | 1.5209 | 
| Refractive index* nC | 1.5204 | 
| Abbe value νe | 55 | 
| Photoelastic constant in (nm/cm)/Mpa | 34.7 | 
* Refractive indices: Pretreatment of samples.
Condition as supplied ["as drawn"].
2. Thermal properties
| Thermal Properties - General | Unit | Value | 
|---|---|---|
| CTE (Coefficient of thermal expansion) α | 10-6·K-1 (20 °C; 300 °C) | 7.2 | 
| Mean specific heat capacity cp | J/(g·K) (20 °C to 100 °C) | 0.8 | 
| Transformation temperature Tg | °C | 557 | 
| Thermal Properties - Viscosities | Viscosity lg ŋ in dPas | Temperature in °C | 
|---|---|---|
| Strain point | 14.5 | 529 | 
| Annealing point | 13.0 | 557 | 
| Softening point | 7.6 | 736 | 
3. Mechanical properties
| Mechanical Properties | 
            Unit | Value | 
|---|---|---|
| Density ρ | in g/cm³ | 2.51 | 
| Young's modulus E | in kN/mm² | 72.9 | 
| Poisson's ratio µ | 0.21 | |
| Torsion modulus G | in kN/mm² | 30 | 
| Knoop hardness | HK 0.1/20 | 470 | 
| Vickers hardness | HV 0.2/25 | 510 | 
Chemical toughening (for thickness = 0.3 mm)
| Unit | 
            Value | 
|---|---|
| Temperature ϑ in °C | 410 | 
| Time t in h | 4 | 
| Compressive stress (CS) in MPa | 320 | 
| Depth of layer (DoL) in µm | 18 | 
4. Chemical properties
| Hydrolytic resistance (acc. to DIN ISO 719) | Value | 
|---|---|
| Class | HGB 1 | 
| Equivalent of alkali per gram glass grains in µg/g | 20 | 
| Acid resistance (acc. to DIN 12116) | Value | 
|---|---|
| Class | S 2 | 
| Half surface weight loss after 6 hours in mg/dm² | 1.4 | 
| Alkali resistance (acc. to DIN ISO 695) | Value | 
|---|---|
| Class | A 2 | 
| Surface weight loss after 3 hours in mg/dm² | 88 | 
5. Electrical properties
| Dielectric constant εr (at ϑ = 25 °C) | Value | 
|---|---|
| at 1 MHz | 6.7 | 
| at 1 GHz | 6.4 | 
| at 5 GHz | 6.3 | 
| Dissipation factor tan δ (at ϑ = 25 °C) | 
            Value | 
|---|---|
| at 1 MHz | 61·10-4 | 
| at 1 GHz | 74·10-4 | 
| at 5 GHz | 101·10-4 | 
| Electric volume resistivity ρD in Ω·cm (at 50 Hz) | 
        
|---|
| 1.6·108 ( ϑ = 250 °C) | 
| 3.5·106 (ϑ = 350 °C) | 
6. Transmittance values
| Wavelength in nm at thickness 0.3 mm: | τ (λ) in % | 
|---|---|
| 254 | < 0.1 | 
| 380 | 91.2 | 
        
| 632.8 | 92.0 | 
        
| 1064 | 92.0 | 
        
| Edge wavelength λc (τ = 0.46) at thickness in mm | Wavelength in nm | 
|---|---|
| 0.10 | 308 | 
| 0.21 | 315 | 
| 0.30 | 318 | 
| 0.40 | 321 | 
| 1.10 | 329 | 
| Luminous transmittance at thickness in mm | τvD65in % | 
|---|---|
| 0.3 | 91.7 ± 0.3 | 
D 263® products
SCHOTT D 263® is available as:
- Sheets
 - Cut-to-size substrates
 - Unpolished substrates and wafers