技术规格
内部透过率(图表)
- SCHOTT
- RG80 - RG80
- 厚度
- 1.0
- 反射系数
- 0.9071
内部透过率(表格)
| λ [nm] | |
|---|---|
| 200 | < 10⁻³ |
| 210 | < 10⁻³ |
| 220 | < 10⁻³ |
| 230 | < 10⁻³ |
| 240 | < 10⁻³ |
| 250 | < 10⁻³ |
| 260 | < 10⁻³ |
| 270 | < 10⁻³ |
| 280 | < 10⁻³ |
| 290 | < 10⁻³ |
| 300 | < 10⁻³ |
| 310 | < 10⁻³ |
| 320 | < 10⁻³ |
| 330 | < 10⁻³ |
| 340 | < 10⁻³ |
| 350 | < 10⁻³ |
| 360 | < 10⁻³ |
| 370 | < 10⁻³ |
| 380 | < 10⁻³ |
| 390 | < 10⁻³ |
| 400 | < 10⁻³ |
| 410 | < 10⁻³ |
| 420 | < 10⁻³ |
| 430 | < 10⁻³ |
| 440 | < 10⁻³ |
| 450 | < 10⁻³ |
| 460 | < 10⁻³ |
| 470 | < 10⁻³ |
| 480 | < 10⁻³ |
| 490 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 500 | < 10⁻³ |
| 510 | < 10⁻³ |
| 520 | < 10⁻³ |
| 530 | < 10⁻³ |
| 540 | < 10⁻³ |
| 550 | < 10⁻³ |
| 560 | < 10⁻³ |
| 570 | < 10⁻³ |
| 580 | < 10⁻³ |
| 590 | < 10⁻³ |
| 600 | < 10⁻³ |
| 610 | < 10⁻³ |
| 620 | < 10⁻³ |
| 630 | < 10⁻³ |
| 640 | < 10⁻³ |
| 650 | < 10⁻³ |
| 660 | < 10⁻³ |
| 670 | < 10⁻³ |
| 680 | < 10⁻³ |
| 690 | < 10⁻³ |
| 700 | < 10⁻³ |
| 710 | 0.001 |
| 720 | 0.007 |
| 730 | 0.021 |
| 740 | 0.040 |
| 750 | 0.062 |
| 760 | 0.093 |
| 770 | 0.151 |
| 780 | 0.262 |
| 790 | 0.428 |
| λ [nm] | |
|---|---|
| 800 | 0.603 |
| 810 | 0.735 |
| 820 | 0.809 |
| 830 | 0.843 |
| 840 | 0.851 |
| 850 | 0.851 |
| 860 | 0.844 |
| 870 | 0.826 |
| 880 | 0.810 |
| 890 | 0.790 |
| 900 | 0.773 |
| 910 | 0.751 |
| 920 | 0.728 |
| 930 | 0.703 |
| 940 | 0.677 |
| 950 | 0.649 |
| 960 | 0.620 |
| 970 | 0.587 |
| 980 | 0.553 |
| 990 | 0.517 |
| 1,000 | 0.479 |
| 1,010 | 0.439 |
| 1,020 | 0.398 |
| 1,030 | 0.356 |
| 1,040 | 0.315 |
| 1,050 | 0.274 |
| 1,060 | 0.235 |
| 1,070 | 0.199 |
| 1,080 | 0.165 |
| 1,090 | 0.135 |
| λ [nm] | |
|---|---|
| 1,100 | 0.109 |
| 1,110 | 0.086 |
| 1,120 | 0.067 |
| 1,130 | 0.052 |
| 1,140 | 0.040 |
| 1,150 | 0.030 |
| 1,160 | 0.023 |
| 1,170 | 0.017 |
| 1,180 | 0.013 |
| 1,190 | 0.010 |
| 1,200 | 0.008 |
| 1,250 | 0.003 |
| 1,300 | 0.002 |
| 1,350 | 0.002 |
| 1,400 | 0.002 |
| 1,450 | 0.001 |
| 1,500 | 0.001 |
| 1,550 | 0.002 |
| 1,600 | 0.003 |
| 1,650 | 0.003 |
| 1,700 | 0.003 |
| 1,750 | 0.003 |
| 1,800 | 0.004 |
| 1,850 | 0.007 |
| 1,900 | 0.013 |
| 1,950 | 0.024 |
| 2,000 | 0.038 |
| 2,050 | 0.054 |
| 2,100 | 0.072 |
| 2,150 | 0.095 |
| λ [nm] | |
|---|---|
| 2,200 | 0.123 |
| 2,250 | 0.155 |
| 2,300 | 0.190 |
| 2,350 | 0.223 |
| 2,400 | 0.251 |
| 2,450 | 0.273 |
| 2,500 | 0.286 |
| 2,550 | |
| 2,600 | |
| 2,650 | |
| 2,700 | |
| 2,750 | |
| 2,800 | |
| 2,850 | |
| 2,900 | |
| 2,950 | |
| 3,000 | |
| 3,050 | |
| 3,100 | |
| 3,150 | |
| 3,200 | |
| 3,250 | |
| 3,300 | |
| 3,350 | |
| 3,400 | |
| 3,450 | |
| 3,500 | |
| 3,550 | |
| 3,600 | |
| 3,650 | |
| λ [nm] | |
|---|---|
| 3,700 | |
| 3,750 | |
| 3,800 | |
| 3,850 | |
| 3,900 | |
| 3,950 | |
| 4,000 | |
| 4,050 | |
| 4,100 | |
| 4,150 | |
| 4,200 | |
| 4,250 | |
| 4,300 | |
| 4,350 | |
| 4,400 | |
| 4,450 | |
| 4,500 | |
| 4,550 | |
| 4,600 | |
| 4,650 | |
| 4,700 | |
| 4,750 | |
| 4,800 | |
| 4,850 | |
| 4,900 | |
| 4,950 | |
| 5,000 | |
| 5,050 | |
| 5,100 | |
| 5,150 | |
光学值
| 反射系数 | |
|---|---|
| Pd | 0.907 |
| 参考厚度 | |
|---|---|
| d [mm] | 1 |
| 折射率 n |
|---|
| nF (486.1 nm) = 1.574 |
| nh (404.7 nm) = 1.586 |
| ng (435.8 nm) = 1.581 |
| ns (852.1 nm) = 1.557 |
| ne (546.1 nm) = 1.569 |
| nd (587.6 nm) = 1.566 |
色度评估
| 光源 | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
| 光源 | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
| 光源 | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
物理值
| 密度 | |
|---|---|
| p [g/cm3] | 2.9854 |
| 气泡含量 | |
|---|---|
| 气泡等级 | |
| 玻转温度 | |
|---|---|
| Tg [°C] | 543 |
| 温度系数 | |
|---|---|
| Tk [nm/°C] | |
| 耐化学性 | |
|---|---|
| 耐污性 | 5 |
| 耐酸性 | 53.4 |
| 耐碱性 | 1.3 |
| 热膨胀 | |
|---|---|
| α-30°C/+70°C [10-6/K] | |
| α20°C/300°C [10-6/K] | 10.25 |
| α20°C/200°C [10-6/K] | |