玻璃类型 |
物品编号 |
长度 |
宽度 |
厚度 |
重量 |
---|
KG5
- SCHOTT
- KG5 - KG5
- 厚度
- 2.0
- 反射系数
- 0.9200
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | 0.002 |
300 | 0.022 |
310 | 0.114 |
320 | 0.295 |
330 | 0.516 |
340 | 0.684 |
350 | 0.795 |
360 | 0.869 |
370 | 0.898 |
380 | 0.909 |
390 | 0.900 |
400 | 0.877 |
410 | 0.862 |
420 | 0.850 |
430 | 0.850 |
440 | 0.862 |
450 | 0.865 |
460 | 0.862 |
470 | 0.872 |
480 | 0.879 |
490 | 0.884 |
λ [nm] | |
---|---|
500 | 0.888 |
510 | 0.885 |
520 | 0.878 |
530 | 0.874 |
540 | 0.881 |
550 | 0.890 |
560 | 0.892 |
570 | 0.887 |
580 | 0.877 |
590 | 0.860 |
600 | 0.838 |
610 | 0.810 |
620 | 0.777 |
630 | 0.738 |
640 | 0.696 |
650 | 0.650 |
660 | 0.604 |
670 | 0.555 |
680 | 0.505 |
690 | 0.450 |
700 | 0.398 |
710 | 0.347 |
720 | 0.299 |
730 | 0.255 |
740 | 0.214 |
750 | 0.178 |
760 | 0.145 |
770 | 0.116 |
780 | 0.092 |
790 | 0.072 |
λ [nm] | |
---|---|
800 | 0.056 |
810 | 0.042 |
820 | 0.032 |
830 | 0.023 |
840 | 0.016 |
850 | 0.011 |
860 | 0.008 |
870 | 0.005 |
880 | 0.004 |
890 | 0.003 |
900 | 0.002 |
910 | 0.001 |
920 | 0.001 |
930 | < 10⁻³ |
940 | < 10⁻³ |
950 | < 10⁻³ |
960 | < 10⁻³ |
970 | < 10⁻³ |
980 | < 10⁻³ |
990 | < 10⁻³ |
1,000 | < 10⁻³ |
1,010 | < 10⁻³ |
1,020 | < 10⁻³ |
1,030 | < 10⁻³ |
1,040 | < 10⁻³ |
1,050 | < 10⁻³ |
1,060 | < 10⁻³ |
1,070 | < 10⁻³ |
1,080 | < 10⁻³ |
1,090 | < 10⁻³ |
λ [nm] | |
---|---|
1,100 | < 10⁻³ |
1,110 | < 10⁻³ |
1,120 | < 10⁻³ |
1,130 | < 10⁻³ |
1,140 | < 10⁻³ |
1,150 | < 10⁻³ |
1,160 | < 10⁻³ |
1,170 | < 10⁻³ |
1,180 | < 10⁻³ |
1,190 | < 10⁻³ |
1,200 | < 10⁻³ |
1,250 | < 10⁻³ |
1,300 | < 10⁻³ |
1,350 | < 10⁻³ |
1,400 | < 10⁻³ |
1,450 | < 10⁻³ |
1,500 | < 10⁻³ |
1,550 | < 10⁻³ |
1,600 | < 10⁻³ |
1,650 | < 10⁻³ |
1,700 | < 10⁻³ |
1,750 | < 10⁻³ |
1,800 | < 10⁻³ |
1,850 | < 10⁻³ |
1,900 | < 10⁻³ |
1,950 | < 10⁻³ |
2,000 | < 10⁻³ |
2,050 | < 10⁻³ |
2,100 | < 10⁻³ |
2,150 | < 10⁻³ |
λ [nm] | |
---|---|
2,200 | < 10⁻³ |
2,250 | < 10⁻³ |
2,300 | < 10⁻³ |
2,350 | 0.001 |
2,400 | 0.001 |
2,450 | 0.002 |
2,500 | 0.003 |
2,550 | 0.004 |
2,600 | 0.005 |
2,650 | 0.007 |
2,700 | 0.008 |
2,750 | 0.006 |
2,800 | < 10⁻³ |
2,850 | < 10⁻³ |
2,900 | < 10⁻³ |
2,950 | < 10⁻³ |
3,000 | < 10⁻³ |
3,050 | < 10⁻³ |
3,100 | < 10⁻³ |
3,150 | < 10⁻³ |
3,200 | < 10⁻³ |
3,250 | < 10⁻³ |
3,300 | < 10⁻³ |
3,350 | < 10⁻³ |
3,400 | < 10⁻³ |
3,450 | < 10⁻³ |
3,500 | < 10⁻³ |
3,550 | 0.001 |
3,600 | 0.002 |
3,650 | 0.002 |
λ [nm] | |
---|---|
3,700 | 0.002 |
3,750 | 0.002 |
3,800 | 0.002 |
3,850 | 0.001 |
3,900 | < 10⁻³ |
3,950 | < 10⁻³ |
4,000 | < 10⁻³ |
4,050 | < 10⁻³ |
4,100 | < 10⁻³ |
4,150 | < 10⁻³ |
4,200 | < 10⁻³ |
4,250 | < 10⁻³ |
4,300 | < 10⁻³ |
4,350 | < 10⁻³ |
4,400 | < 10⁻³ |
4,450 | < 10⁻³ |
4,500 | < 10⁻³ |
4,550 | < 10⁻³ |
4,600 | < 10⁻³ |
4,650 | < 10⁻³ |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.920 |
参考厚度 | |
---|---|
d [mm] | 2 |
承诺光谱值 | |
---|---|
τi (365nm) | ≥0.8 |
τi (500nm) | ≥0.86 |
τi (600nm) | ≥0.8 |
τi (700nm) | ≤0.43 |
τi (800nm) | ≤0.09 |
τi (900nm) | ≤0.008 |
τi (1060nm) | ≤0.0001 |
τi (2200nm) | ≤0.001 |
折射率 n |
---|
nF (486.1 nm) = 1.518 |
nh (404.7 nm) = 1.526 |
ng (435.8 nm) = 1.523 |
ns (852.1 nm) = 1.506 |
ne (546.1 nm) = 1.515 |
nd (587.6 nm) = 1.513 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.440 | 0.434 | 0.427 |
y | 0.411 | 0.415 | 0.418 |
Y | 85 | 78 | 72 |
λd [nm] | 504 | 505 | 505 |
Pe | 0.02 | 0.03 | 0.05 |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.416 | 0.410 | 0.404 |
y | 0.402 | 0.406 | 0.409 |
Y | 85 | 78 | 72 |
λd [nm] | 503 | 503 | 503 |
Pe | 0.02 | 0.03 | 0.05 |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.308 | 0.304 | 0.300 |
y | 0.331 | 0.332 | 0.334 |
Y | 85 | 79 | 74 |
λd [nm] | 496 | 496 | 496 |
Pe | 0.02 | 0.03 | 0.04 |
密度 | |
---|---|
p [g/cm3] | 2.53 |
气泡含量 | |
---|---|
气泡等级 | 3 |
玻转温度 | |
---|---|
Tg [°C] | 565 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 3.0 |
耐碱性 | 4.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 5.4 |
α20°C/300°C [10-6/K] | 6.2 |
α20°C/200°C [10-6/K] |