一种耐高湿度的近红外截至滤色片。
在下面的标签或我们的 网页上查找更多的信息。
使用 交互式滤色图表和和 滤色计算工具可以找到符合您需求的合适的滤色玻璃。
对于定制的滤色产品,请标记并使用请求按钮。
*典型产品图片展示
技术规格
内部透过率(图表)
- SCHOTT
- BG63 - BG63
- 厚度
- 1.0
- 反射系数
- 0.9160
内部透过率(表格)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | |
| 290 | |
| 300 | < 10⁻³ |
| 310 | 0.002 |
| 320 | 0.070 |
| 330 | 0.327 |
| 340 | 0.619 |
| 350 | 0.809 |
| 360 | 0.902 |
| 370 | 0.944 |
| 380 | 0.964 |
| 390 | 0.975 |
| 400 | 0.980 |
| 410 | 0.983 |
| 420 | 0.985 |
| 430 | 0.987 |
| 440 | 0.988 |
| 450 | 0.990 |
| 460 | 0.991 |
| 470 | 0.992 |
| 480 | 0.992 |
| 490 | 0.992 |
| λ [nm] | |
|---|---|
| 500 | 0.991 |
| 510 | 0.988 |
| 520 | 0.984 |
| 530 | 0.976 |
| 540 | 0.964 |
| 550 | 0.947 |
| 560 | 0.923 |
| 570 | 0.893 |
| 580 | 0.854 |
| 590 | 0.808 |
| 600 | 0.754 |
| 610 | 0.694 |
| 620 | 0.630 |
| 630 | 0.563 |
| 640 | 0.498 |
| 650 | 0.434 |
| 660 | 0.373 |
| 670 | 0.318 |
| 680 | 0.270 |
| 690 | 0.227 |
| 700 | 0.190 |
| 710 | 0.159 |
| 720 | 0.134 |
| 730 | 0.113 |
| 740 | 0.097 |
| 750 | 0.082 |
| 760 | 0.071 |
| 770 | 0.063 |
| 780 | 0.056 |
| 790 | 0.051 |
| λ [nm] | |
|---|---|
| 800 | 0.048 |
| 810 | 0.045 |
| 820 | 0.043 |
| 830 | 0.042 |
| 840 | 0.041 |
| 850 | 0.041 |
| 860 | 0.041 |
| 870 | 0.041 |
| 880 | 0.042 |
| 890 | 0.044 |
| 900 | 0.046 |
| 910 | 0.049 |
| 920 | 0.052 |
| 930 | 0.054 |
| 940 | 0.058 |
| 950 | 0.061 |
| 960 | 0.065 |
| 970 | 0.070 |
| 980 | 0.075 |
| 990 | 0.080 |
| 1,000 | 0.085 |
| 1,010 | 0.093 |
| 1,020 | 0.099 |
| 1,030 | 0.106 |
| 1,040 | 0.112 |
| 1,050 | 0.120 |
| 1,060 | 0.128 |
| 1,070 | 0.135 |
| 1,080 | 0.144 |
| 1,090 | 0.152 |
| λ [nm] | |
|---|---|
| 1,100 | 0.162 |
| 1,110 | 0.171 |
| 1,120 | 0.181 |
| 1,130 | 0.191 |
| 1,140 | 0.202 |
| 1,150 | 0.212 |
| 1,160 | 0.224 |
| 1,170 | 0.235 |
| 1,180 | 0.247 |
| 1,190 | 0.259 |
| 1,200 | 0.273 |
| 1,250 | 0.340 |
| 1,300 | 0.412 |
| 1,350 | 0.484 |
| 1,400 | 0.548 |
| 1,450 | 0.614 |
| 1,500 | 0.675 |
| 1,550 | 0.727 |
| 1,600 | 0.770 |
| 1,650 | 0.808 |
| 1,700 | 0.839 |
| 1,750 | 0.863 |
| 1,800 | 0.882 |
| 1,850 | 0.899 |
| 1,900 | 0.911 |
| 1,950 | 0.920 |
| 2,000 | 0.928 |
| 2,050 | 0.934 |
| 2,100 | 0.939 |
| 2,150 | 0.941 |
| λ [nm] | |
|---|---|
| 2,200 | 0.941 |
| 2,250 | 0.939 |
| 2,300 | 0.939 |
| 2,350 | 0.939 |
| 2,400 | 0.939 |
| 2,450 | 0.936 |
| 2,500 | 0.932 |
| 2,550 | 0.935 |
| 2,600 | 0.928 |
| 2,650 | 0.921 |
| 2,700 | 0.910 |
| 2,750 | 0.888 |
| 2,800 | 0.809 |
| 2,850 | 0.681 |
| 2,900 | 0.573 |
| 2,950 | 0.494 |
| 3,000 | 0.433 |
| 3,050 | 0.379 |
| 3,100 | 0.330 |
| 3,150 | 0.286 |
| 3,200 | 0.249 |
| 3,250 | 0.219 |
| 3,300 | 0.195 |
| 3,350 | 0.177 |
| 3,400 | 0.164 |
| 3,450 | 0.156 |
| 3,500 | 0.153 |
| 3,550 | 0.156 |
| 3,600 | 0.163 |
| 3,650 | 0.175 |
| λ [nm] | |
|---|---|
| 3,700 | 0.192 |
| 3,750 | 0.209 |
| 3,800 | 0.217 |
| 3,850 | 0.206 |
| 3,900 | 0.180 |
| 3,950 | 0.149 |
| 4,000 | 0.111 |
| 4,050 | 0.067 |
| 4,100 | 0.035 |
| 4,150 | 0.017 |
| 4,200 | 0.009 |
| 4,250 | 0.006 |
| 4,300 | 0.006 |
| 4,350 | 0.007 |
| 4,400 | 0.007 |
| 4,450 | 0.005 |
| 4,500 | 0.004 |
| 4,550 | 0.004 |
| 4,600 | 0.004 |
| 4,650 | 0.005 |
| 4,700 | 0.008 |
| 4,750 | 0.015 |
| 4,800 | 0.023 |
| 4,850 | 0.031 |
| 4,900 | 0.041 |
| 4,950 | 0.054 |
| 5,000 | 0.068 |
| 5,050 | 0.081 |
| 5,100 | 0.089 |
| 5,150 | 0.092 |
光学值
| 反射系数 | |
|---|---|
| Pd | 0.916 |
| 参考厚度 | |
|---|---|
| d [mm] | 1 |
| 承诺光谱值 | |
|---|---|
| τi (405nm) | ≥0.95 |
| τi (514nm) | ≥0.96 |
| τi (633nm) | ≥0.5 |
| τi (694nm) | ≤0.25 |
| τi (1060nm) | ≤0.16 |
| 折射率 n |
|---|
| nF (486.1 nm) = 1.538 |
| nh (404.7 nm) = 1.546 |
| ng (435.8 nm) = 1.542 |
| ns (852.1 nm) = 1.525 |
| ne (546.1 nm) = 1.534 |
| nd (587.6 nm) = 1.532 |
色度评估
| 光源 | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.403 | 0.366 | 0.336 |
| y | 0.420 | 0.428 | 0.432 |
| Y | 76 | 66 | 59 |
| λd [nm] | 500 | 499 | 499 |
| Pe | 0.10 | 0.19 | 0.26 |
| 光源 | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.380 | 0.344 | 0.316 |
| y | 0.408 | 0.412 | 0.414 |
| Y | 77 | 68 | 60 |
| λd [nm] | 498 | 497 | 497 |
| Pe | 0.11 | 0.19 | 0.27 |
| 光源 | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.280 | 0.255 | 0.237 |
| y | 0.325 | 0.319 | 0.313 |
| Y | 81 | 73 | 67 |
| λd [nm] | 490 | 489 | 489 |
| Pe | 0.12 | 0.22 | 0.29 |
物理值
| 密度 | |
|---|---|
| p [g/cm3] | 2.7855 |
| 气泡含量 | |
|---|---|
| 气泡等级 | |
| 玻转温度 | |
|---|---|
| Tg [°C] | 416 |
| 温度系数 | |
|---|---|
| Tk [nm/°C] | |
| 耐化学性 | |
|---|---|
| 耐污性 | 1.0 |
| 耐酸性 | 52.3 |
| 耐碱性 | 3.3 |
| 热膨胀 | |
|---|---|
| α-30°C/+70°C [10-6/K] | 11.91 |
| α20°C/300°C [10-6/K] | 13.93 |
| α20°C/200°C [10-6/K] | |