Please note: Due to maintenance the shop will be unavailable on Tuesday, November 30, from 06:00 AM until 08:00 AM (CEST)

P-LAF37  755457.399

optical glass klein 4zu3.jpg
特性
nd 1.75550 νd 45.66
ne 1.75944 νe 45.42
nF-nC 0.016546 nF'-nC' 0.016722
特性 λ [nm]
n2,325.4 2,325.4 1.71338
n1,970.1 1,970.1 1.72058
n1,529.6 1,529.6 1.72830
n1,060.0 1,060.0 1.73669
nt 1,014.0 1.73770
ns 852.1 1.74198
nr 706.5 1.74775
nC 656.3 1.75054
nC' 643.8 1.75132
特性 λ [nm]
n632.8 632.8 1.75206
nD 589.3 1.75535
nd 587.6 1.75550
ne 546.1 1.75944
nF 486.1 1.76708
nF' 480.0 1.76804
ng 435.8 1.77633
nh 404.7 1.78414
ni 365.0
特性 λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
特性 λ [nm]
τ25/2500 2,500 0.160
τ25/2325 2,325 0.490
τ25/1970 1,970 0.870
τ25/1530 1,530 0.976
τ25/1060 1,060 0.996
τ25/700 700 0.996
τ25/660 660 0.995
τ25/620 620 0.994
τ25/580 580 0.994
τ25/546 546 0.994
τ25/500 500 0.991
τ25/460 460 0.983
τ25/436 436 0.975
τ25/420 420 0.967
τ25/405 405 0.955
τ25/400 400 0.950
τ25/390 390 0.930
τ25/380 380 0.900
τ25/370 370 0.845
τ25/365 365 0.810
τ25/350 350 0.640
τ25/334 334 0.340
τ25/320 320 0.040
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
特性 λ [nm]
τ10/2500 2,500 0.480
τ10/2325 2,325 0.752
τ10/1970 1,970 0.946
τ10/1530 1,530 0.990
τ10/1060 1,060 0.998
τ10/700 700 0.998
τ10/660 660 0.998
τ10/620 620 0.998
τ10/580 580 0.998
τ10/546 546 0.998
τ10/500 500 0.996
τ10/460 460 0.993
τ10/436 436 0.990
τ10/420 420 0.987
τ10/405 405 0.982
τ10/400 400 0.980
τ10/390 390 0.971
τ10/380 380 0.959
τ10/370 370 0.935
τ10/365 365 0.919
τ10/350 350 0.837
τ10/334 334 0.650
τ10/320 320 0.276
τ10/310 310 0.040
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
特性
Ps,t 0.2591
PC,s 0.5170
Pd,C 0.2999
Pe,d 0.2379
Pg,F 0.5590
Pi,h
P's,t 0.2563
P'C',s 0.5585
P'd,C' 0.2498
P'e,d 0.2354
P'g,F' 0.4957
P'i,h
特性
ΔPC,t 0.0145
ΔPC,s 0.0077
ΔPF,e -0.0022
ΔPg,F -0.0080
ΔPi,g