技术规格
        
            折射率
        
| 特性 | λ [nm] | |
|---|---|---|
| n2,325.4 | 2,325.4 | 1.44114 | 
| n1,970.1 | 1,970.1 | 1.44388 | 
| n1,529.6 | 1,529.6 | 1.44683 | 
| n1,060.0 | 1,060.0 | 1.44991 | 
| nt | 1,014.0 | 1.45026 | 
| ns | 852.1 | 1.45171 | 
| nr | 706.5 | 1.45358 | 
| nC | 656.3 | 1.45446 | 
| nC' | 643.8 | 1.45471 | 
| 特性 | λ [nm] | |
|---|---|---|
| n632.8 | 632.8 | 1.45494 | 
| nD | 589.3 | 1.45596 | 
| nd | 587.6 | 1.45600 | 
| ne | 546.1 | 1.45720 | 
| nF | 486.1 | 1.45948 | 
| nF' | 480.0 | 1.45976 | 
| ng | 435.8 | 1.46216 | 
| nh | 404.7 | 1.46436 | 
| ni | 365.0 | 1.46807 | 
| 特性 | λ [nm] | |
|---|---|---|
| n334.1 | 334.1 | 1.47199 | 
| n312.6 | 312.6 | |
| n296.7 | 296.7 | |
| n280.4 | 280.4 | |
| n248.3 | 248.3 | |
        
            内部透射率
        
| 特性 | λ [nm] | |
|---|---|---|
| τ25/2500 | 2,500 | 0.993 | 
| τ25/2325 | 2,325 | 0.996 | 
| τ25/1970 | 1,970 | 0.998 | 
| τ25/1530 | 1,530 | 0.998 | 
| τ25/1060 | 1,060 | 0.995 | 
| τ25/700 | 700 | 0.993 | 
| τ25/660 | 660 | 0.993 | 
| τ25/620 | 620 | 0.994 | 
| τ25/580 | 580 | 0.994 | 
| τ25/546 | 546 | 0.995 | 
| τ25/500 | 500 | 0.994 | 
| τ25/460 | 460 | 0.992 | 
| τ25/436 | 436 | 0.991 | 
| τ25/420 | 420 | 0.991 | 
| τ25/405 | 405 | 0.991 | 
| τ25/400 | 400 | 0.991 | 
| τ25/390 | 390 | 0.990 | 
| τ25/380 | 380 | 0.987 | 
| τ25/370 | 370 | 0.980 | 
| τ25/365 | 365 | 0.975 | 
| τ25/350 | 350 | 0.940 | 
| τ25/334 | 334 | 0.830 | 
| τ25/320 | 320 | 0.610 | 
| τ25/310 | 310 | 0.400 | 
| τ25/300 | 300 | 0.200 | 
| τ25/290 | 290 | 0.080 | 
| τ25/280 | 280 | 0.028 | 
| τ25/270 | 270 | 0.010 | 
| τ25/260 | 260 | 0.005 | 
| τ25/250 | 250 | |
| 特性 | λ [nm] | |
|---|---|---|
| τ10/2500 | 2,500 | 0.997 | 
| τ10/2325 | 2,325 | 0.998 | 
| τ10/1970 | 1,970 | 0.999 | 
| τ10/1530 | 1,530 | 0.999 | 
| τ10/1060 | 1,060 | 0.998 | 
| τ10/700 | 700 | 0.997 | 
| τ10/660 | 660 | 0.997 | 
| τ10/620 | 620 | 0.997 | 
| τ10/580 | 580 | 0.998 | 
| τ10/546 | 546 | 0.998 | 
| τ10/500 | 500 | 0.998 | 
| τ10/460 | 460 | 0.997 | 
| τ10/436 | 436 | 0.996 | 
| τ10/420 | 420 | 0.996 | 
| τ10/405 | 405 | 0.996 | 
| τ10/400 | 400 | 0.996 | 
| τ10/390 | 390 | 0.996 | 
| τ10/380 | 380 | 0.995 | 
| τ10/370 | 370 | 0.992 | 
| τ10/365 | 365 | 0.990 | 
| τ10/350 | 350 | 0.976 | 
| τ10/334 | 334 | 0.928 | 
| τ10/320 | 320 | 0.821 | 
| τ10/310 | 310 | 0.693 | 
| τ10/300 | 300 | 0.525 | 
| τ10/290 | 290 | 0.364 | 
| τ10/280 | 280 | 0.239 | 
| τ10/270 | 270 | 0.152 | 
| τ10/260 | 260 | 0.109 | 
| τ10/250 | 250 | 0.090 | 
        
            部分色散
        
| 特性 | |
|---|---|
| Ps,t | 0.2894 | 
| PC,s | 0.5481 | 
| Pd,C | 0.3066 | 
| Pe,d | 0.2388 | 
| Pg,F | 0.5347 | 
| Pi,h | 0.7387 | 
| P's,t | 0.2873 | 
| P'C',s | 0.5927 | 
| P'd,C' | 0.2557 | 
| P'e,d | 0.2371 | 
| P'g,F' | 0.4749 | 
| P'i,h | 0.7334 | 
| 特性 | |
|---|---|
| ΔPC,t | -0.1386 | 
| ΔPC,s | -0.0667 | 
| ΔPF,e | 0.0140 | 
| ΔPg,F | 0.0438 | 
| ΔPi,g | 0.2157 | 
下载
产品目录
TIE's - 技术信息
                                        TIE-04: Test Report for Delivery Lots of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            230 kB
                                    
                                        TIE-19: Temperature Coefficient of the Refractive Index (EN)
                                    
                                    
                                            PDF 
                                            450 kB
                                    
                                        TIE-25: Striae in Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            1.24 MB
                                    
                                        TIE-26: Homogeneity of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            990 kB
                                    
                                        TIE-27: Stress in Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            710 kB
                                    
                                        TIE-28: Bubbles and Inclusions in Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            260 kB
                                    
                                        TIE-30: Chemical Properties of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            210 kB
                                    
                                        TIE-31: Mechanical and Thermal Properties of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            190 kB
                                    
                                        TIE-32: Thermal Loads on Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            100 kB
                                    
                                        TIE-33: Bending Strength of Optical Glass and ZERODUR® (EN)
                                    
                                    
                                            PDF 
                                            2.76 MB
                                    
                                        TIE-35: Transmittance of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            510 kB
                                    
                                        TIE-36: Fluorescence of Optical Glass (EN)
                                    
                                    
                                            PDF 
                                            710 kB
                                    
                                        TIE-40: Optical Glass for Precision Molding (EN)
                                    
                                    
                                            PDF 
                                            610 kB
                                    
                                        TIE-41: Large Optical Glass Blanks (EN)
                                    
                                    
                                            PDF 
                                            2.06 MB
                                    